What C26000 Cartridge Brass Is
C26000 is a copper-zinc alloy with about 70% copper and 30% zinc, known in European practice as CuZn30 and traditionally as cartridge brass because it was developed for deep-drawn ammunition cases. In the Chinese designation system its composition corresponds to the grade H70 in GB/T 5231. It has the highest ductility of the yellow brass series and is the material of choice whenever a component must be formed deeply without cracking.
The alloy is supplied in two broad product families. Cold rolled strip and sheet, in tempers from soft through quarter-hard to full hard, is used for deep drawing, stamping and blanking. Hot rolled plate, strip and rod, produced by rolling or extruding at elevated temperature, is used for heavier sections, for parts that will be machined rather than deep drawn, and as feedstock for further cold reduction. This article deals with both, with emphasis on the hot rolled product.
Chemical Composition
| Element | Requirement % | Comment |
|---|---|---|
| Cu | 68.5-71.5 | the balance of the alloy defines its ductility and colour |
| Fe | 0.05 max | controlled to preserve formability |
| Pb | 0.07 max | kept low; higher lead would improve machinability at the cost of ductility |
| Zn | remainder | principal alloying addition |
ASTM B36 covers plate, sheet, strip and rolled bar in C26000; ASTM B19 covers rod and bar; ASTM B134 covers wire; ASTM B135 covers seamless brass tube; and ASTM B587 covers welded brass tube. The same composition is quoted as H70 in GB/T 5231 and as CuZn30 in the European designation system, so a single heat can normally be certified against several standards.
Mechanical and Physical Properties
| Property | Value or behaviour |
|---|---|
| Density | 8.53 g/cm³ (0.308 lb/in³) |
| Melting range | approximately 915-955 C |
| Modulus of elasticity | approximately 110 GPa (16 x 10^6 psi) |
| Electrical conductivity | approximately 28% IACS, with electrical resistivity of about 6.2 microhm-cm at 20 C |
| Cold working | rated excellent; the alloy work-hardens predictably and responds well to inter-annealing |
| Hot working | rated fair; hot rolling and extrusion are practical within a controlled temperature window |
| Machinability | about 30% of the rating of free-cutting brass, so it is machined rather than freely machined |
| Magnetic behaviour | non-magnetic |
The physical data explain the two operating limits of the grade. Its conductivity is the lowest of the common brasses, which is unimportant for cartridge cases and heat exchanger shells but rules it out of electrical conduction duties. Its machinability is modest, which is the price paid for the ductility that makes the alloy valuable for drawing.
Hot Rolling Practice and Temper Selection
Hot working of C26000 is carried out in the upper part of the brass working range, in the region of 700-850 C. The window is narrower than for the free-cutting brasses because the low lead content gives less internal lubrication, and the alloy must not be worked below the point at which it becomes brittle. Rolling schedules therefore control both entry and exit temperature carefully, and the hot rolled product is normally pickled to remove surface oxide before being shipped or before further cold reduction.
Annealing between operations is carried out at moderate temperature, in the region of 425-700 C, with the exact cycle chosen to produce a grain size suited to the next forming step. Grain size control is the key process variable for deep drawing: too coarse a grain gives a rough orange-peel surface, while too fine a grain reduces ductility. For drawing stock, grain size is often specified explicitly alongside the temper.
Corrosion Behaviour
C26000 performs well in ordinary atmospheres, fresh water and many neutral chemical environments, and it is widely used in plumbing and heat transfer applications for that reason. Its known limitation is dezincification: in stagnant or aggressive waters, particularly those with high chloride content, high temperature or low flow, the alloy can lose zinc selectively. Where that risk exists, an inhibited brass containing a small controlled arsenic addition - the C26130 type of composition - should be specified instead.
The second classic failure mode is stress-corrosion cracking in ammoniacal or amine-bearing environments. Cold worked parts that carry residual tensile stress are vulnerable, which is why stress relief is specified after severe forming and why fabricated parts should be protected during storage and transport from ammonia sources and their compounds.
Typical Applications
Deep-drawn cartridge cases, shells and ammunition components.
Radiator cores, tanks and heat exchanger shells and tubing.
Plumbing fittings, valves, couplings and general hardware.
Fasteners, snap fasteners, eyelets and zip fastener components.
Lamp fixtures, decorative trim, nameplates, badges and architectural hardware.
Pressed and spun holloware, instrument housings and drawn cans.
Fabrication and Joining Guidance
Cold forming is the strength of the alloy, and the process is best planned around the work-hardening curve: draw, then anneal, then draw again, rather than attempting a reduction that exceeds the remaining ductility. Blanking and shearing produce clean edges with correctly maintained tooling.
Soldering and brazing are both rated excellent and are the preferred joining methods for assemblies. Fusion welding is considerably more problematic because zinc volatilises from the weld pool, producing porosity and fume; oxyacetylene and gas shielded arc welding are only rated fair, and coated metal arc and seam welding are not recommended. Where welding is unavoidable, low heat input and good ventilation are essential. Machining is straightforward with sharp tooling and positive rakes, but the modest rating means feeds and speeds should be set for a ductile brass rather than for a free-cutting grade.
Inspection Points and Common Pitfalls
Verify copper and zinc content on the certificate; the 68.5-71.5% copper window is narrow and a drifting analysis changes formability.
Check grain size and temper against the planned drawing operation, and ask for grain size to be reported for drawing stock.
Confirm the reported conductivity or resistivity, since a figure far from about 28% IACS indicates either a different alloy or an error in the datasheet.
Require visual and dimensional inspection of hot rolled product after pickling; residual scale damages tooling downstream.
Protect cold worked parts from ammonia and moisture during storage to avoid stress-corrosion cracking before the parts enter service.
FAQ
Q: Why is C26000 called cartridge brass?
The name comes from its traditional use in deep-drawn ammunition cartridge cases. The composition of about 70% copper and 30% zinc gives the highest ductility in the yellow brass range, which is exactly what a severe deep-drawing operation requires.
Q: What is the composition of C26000?
ASTM B36 specifies 68.5-71.5% copper with the balance zinc, a maximum of 0.07% lead and a maximum of 0.05% iron. The same composition appears as H70 in GB/T 5231 and as CuZn30 in the European designation system.
Q: What is the electrical conductivity of C26000?
Approximately 28% IACS, corresponding to an electrical resistivity of about 6.2 microhm-cm at 20 C. This is the lowest conductivity among the common brasses, so the alloy is not selected for electrical conduction.
Q: Is C26000 easy to machine?
No, its machinability rating is only about 30% of that of free-cutting brass. It is normally specified for forming rather than machining, and when it must be machined, sharp tooling and feeds suited to a ductile brass are required.
Q: How is C26000 welded?
Soldering and brazing are rated excellent. Fusion welding is difficult because zinc volatilises from the weld pool, causing porosity and fume; only fair ratings are given for the common fusion processes and some are not recommended at all.
Q: Does C26000 dezincify?
It can do so in stagnant or aggressive waters, particularly with high chlorides and elevated temperature. Where that risk exists, an inhibited brass with a small arsenic addition should be selected instead, and the water chemistry should be reviewed before the grade is fixed.