Nov 15, 2025 Leave a message

ASME SB111 C71500 CuNi 70/30 Heat Exchanger Tube Guide

Material Overview: ASME SB111 C71500 (CuNi 70/30)

ASME SB111 C71500 is the 70/30 copper-nickel grade covered by the seamless condenser tube and ferrule stock specification, and UNS C71500 is the designation that appears on the mill test certificate. The alloy is nominally 70% copper and 30% nickel, which places it in the CuNi 70/30 family together with the CuNi30Mn1Fe designation used in European heat exchanger tube standards. Tubes ordered to ASME SB111 are produced to requirements technically identical to ASTM B111/B111M, so the same heat analysis, tensile testing and non-destructive examination apply whichever designation is written on the purchase order. For pipe and tube sizes outside the condenser tube range, the same composition is covered by ASTM B466/B466M.

SB111 C71500 heat exchanger tube is selected where a unit must survive flowing seawater, brackish water or mildly acidic process streams for decades. Moderate thermal conductivity, high resistance to impingement attack and stress corrosion cracking, and usable strength at elevated temperature make it the standard choice for marine coolers, power station condensers and chemical process exchangers.

Chemical Composition Limits

The table below gives the C71500 limits applied to SB111 tube. Copper is reported as the remainder.

Element Min % Max %
Ni (nickel) 29.0 33.0
Fe (iron) 0.40 1.00
Mn (manganese) - 1.00
Zn (zinc) - 1.00
Pb (lead) - 0.05
Cu (copper) Remainder -

Iron and manganese are intentional additions rather than impurities. Iron in the range 0.40-1.00% forms a protective surface film that resists impingement attack in fast-flowing seawater, while manganese improves hot workability and helps stabilise the iron addition. Lead is restricted to 0.05% maximum to protect weldability, and zinc to 1.00% maximum so that the alloy stays inside the corrosion-resistant copper-nickel family.

Physical Properties

Property Metric Imperial
Melting range, solidus to liquidus 1171-1238 °C 2140-2260 °F
Density at 20 °C 8.94 g/cm3 0.323 lb/in3
Electrical conductivity at 20 °C 4.6 % IACS 4.6 % IACS
Thermal conductivity at 20 °C 29 W/(m·K) 17 Btu·ft/(h·ft2·°F)
Coefficient of thermal expansion, 20-300 °C 16.2 x 10-6/K 9 x 10-6/°F
Specific heat capacity at 20 °C 0.377 kJ/(kg·K) 0.09 Btu/(lb·°F)
Modulus of elasticity in tension 152 GPa 22000 ksi
Modulus of rigidity 57 GPa 8300 ksi

The liquidus temperature of 1238 °C and the solidus temperature of 1171 °C give a freezing range of roughly 67 °C, which matters during welding and brazing because the partially molten zone is narrow and solidification cracking is uncommon in this alloy.

Mechanical and Fabrication Data

Representative values for tube in the annealed (O61) and light-drawn (H55) conditions are listed below. Specification minima are stated on the mill certificate for the actual temper supplied.

Tensile strength: approximately 380-550 MPa (55-80 ksi)

0.2% yield strength: approximately 140-380 MPa (20-55 ksi), depending on temper

Elongation: 30% minimum in 50 mm, typically 40% or more in the annealed condition

Machinability rating: about 20% of free-cutting brass, so generous feeds and sharp tooling are used

Cold forming: good, suitable for bending and flaring when the tube is in the annealed temper

Hot forming: good, with working temperatures kept below the annealing range to avoid grain growth

Joining or forming technique Suitability
Soldering Excellent
Brazing Excellent
Oxyacetylene welding Good
Gas shielded arc welding (GTAW/GMAW) Excellent
Coated metal arc welding Excellent
Spot, seam and butt welding Excellent

For fusion welding, a matching nickel-copper filler such as AWS A5.7 ERCuNi is normally used with direct current electrode negative and a shielded trailing gas, because the nickel content of C71500 reduces thermal conductivity and raises weld pool fluidity compared with pure copper. Soldering and brazing are widely used for tube-to-tubesheet joints in condensers.

Corrosion Behaviour and Service Conditions

Among the commercial copper-nickel grades, C71500 offers the highest resistance to aqueous corrosion, covering flowing seawater, brine and diluted non-oxidising acids, and it is highly resistant to stress corrosion cracking and to impingement attack. It also tolerates higher flow velocities than CuNi 90/10, which is why 70/30 tube is specified for the most aggressive circuits of a seawater cooling system.

Two service limits deserve attention. Copper-nickel alloys are sensitive to sulphide-polluted or stagnant seawater, which can strip the protective film; systems should be arranged so that tubes are not left stagnant and are flushed after shutdown. High-temperature strength also falls away above the limits used in pressure vessel design, where CuNi10Fe1Mn is typically restricted to about 300 °C and CuNi30Mn1Fe to about 350 °C, above which creep strength and creep strain limits drop markedly.

Inspection, Testing and Ordering Data

Non-destructive examination: eddy current test on each tube to the specification, with hydrostatic or pneumatic test for tubes above the size threshold

Mechanical tests: tensile test per heat, flattening or expansion test on finished tube

Chemical analysis: heat analysis for nickel, iron, manganese, zinc and lead

Surface condition: clean, free of scale, with ends deburred and capped for transport

Common delivery conditions: annealed O61 or light-drawn H55, in straight lengths up to about 6 m or in U-bent bundles

Identification: heat number and grade marked on each bundle

Specify the grade, temper, outside diameter, wall thickness, length, quantity and any additional testing when ordering, and state whether tubes are to be supplied straight or U-bent for condenser assembly.

Frequently Asked Questions

Q: What is the difference between C71500 and C70600?
C70600 is the CuNi 90/10 grade with 9.0-11.0% nickel and 1.0-1.8% iron, while C71500 contains 29.0-33.0% nickel and 0.40-1.00% iron. The higher nickel content of C71500 gives greater strength, better resistance to impingement and higher tolerable flow velocity, at a correspondingly higher material cost.

Q: Which standard covers SB111 C71500 tube?
ASME SB111 and ASTM B111/B111M cover seamless copper and copper-alloy condenser tubes and ferrule stock. The two documents are technically identical, and C71500 pipe and tube outside condenser tube sizes are also covered by ASTM B466/B466M.

Q: Is ASME SB111 C71500 suitable for seawater service?
Yes. The alloy is widely used for seawater-cooled condensers, shipboard cooling systems and desalination units, provided the seawater is not heavily sulphide-polluted and is kept flowing at a controlled velocity to maintain the protective film.

Q: What are the melting point and maximum service temperature of C71500?
The alloy melts over the range 1171-1238 °C (2140-2260 °F). For pressure equipment, the practical upper limit for CuNi30Mn1Fe is about 350 °C, above which creep strength and creep strain limits fall sharply.

Q: Can C71500 tube be welded or brazed?
Soldering and brazing are rated excellent, as are gas shielded arc, coated metal arc and resistance welding. A matching nickel-copper filler metal such as AWS A5.7 ERCuNi is used for fusion welding, and the annealed temper is preferred for bending and flaring.

Q: How should C71500 tubes be stored and handled?
Keep tubes dry and protected from sulphur-bearing atmospheres, avoid contact with steel racks that can deposit rust and initiate pitting, and cap the ends during transport to protect the bore from contamination.

Send Inquiry

whatsapp

Phone

E-mail

Inquiry