What Is Admiralty Brass Tube?
Admiralty brass is a copper-zinc alloy of the 70/30 family containing small but decisive additions of tin and arsenic. It is designated UNS C44300 in the unified numbering system and CuZn28Sn1 in European practice. The tin addition improves resistance to erosion and impingement attack, while arsenic suppresses the dezincification that plain 70/30 brass would suffer in seawater. That combination is why admiralty brass has remained a default tube material for surface condensers, water coolers and air coolers, and why ASTM B111/B111M and its ASME counterpart ASME SB111 give the alloy a dedicated section.
Seamless tube is produced by hot extrusion of a cast billet followed by cold drawing over a mandrel with intermediate anneals. Because there is no weld seam, the tube carries cooling-water pressure and thermal cycling without a preferential corrosion path. Tubes are supplied in straight lengths or as U-bent tubes for multi-pass exchangers, and may be ordered eddy-current tested for condenser service.
Chemical Composition of UNS C44300
Composition limits are those tabulated for C44300 in ASTM B111/B111M. The alloy is a single-phase alpha brass; the tin and arsenic contents are the elements that govern service performance rather than the mechanical table alone.
| Element | Requirement, % | Function |
|---|---|---|
| Copper (Cu) | 70.0-73.0 | Matrix; thermal conductivity and ductility |
| Tin (Sn) | 0.90-1.20 | Inhibits impingement and erosion attack |
| Arsenic (As) | 0.02-0.06 | Inhibits dezincification |
| Lead (Pb) | 0.07 max | Residual impurity |
| Iron (Fe) | 0.06 max | Residual impurity |
| Zinc (Zn) | Remainder | Balance of the alloy |
| Copper plus named elements | 99.6 min | Sum requirement of the specification |
Other residual elements are held to the low limits stated in the specification; heats are analysed by the manufacturer and the results are reported on the mill certificate.
Mechanical Requirements, Temper and Typical Physical Properties
ASTM B111/B111M sets the tensile requirements by alloy and temper in its property table. Annealed tube, temper O61, is the normal delivery condition for condenser and air cooler service, because it can be expanded into tube sheets and bent to U form without cracking. Hard-drawn tempers are used only for straight tube in low-pressure circuits. Verification is by tension test, expansion or flaring test, and by eddy-current examination when ordered.
| Test or property | Basis of requirement |
|---|---|
| Tensile strength, yield strength, elongation | Property table for C44300 and the ordered temper in ASTM B111/B111M |
| Grain size | Annealed tube examined metallographically against the grain-size limits of the specification |
| Expansion or flare test | Tube expanded over a tapered pin without cracking |
| Eddy-current test | Performed to the acceptance limits of ASTM E243 when specified on the order |
| Hydrostatic or pneumatic test | Applied to the pressure required by the specification |
| Typical physical property | Value, typical for admiralty brass at 20 C |
|---|---|
| Density | 8.53 g/cm³ |
| Thermal conductivity | about 110 W/(m K) |
| Modulus of elasticity | about 110 GPa |
| Melting range | about 900-940 C |
Standard Sizes and Delivery Forms
ASTM B111/B111M covers seamless tube up to 3-1/8 in. outside diameter for condensers, evaporators and heat exchangers. The sizes below reflect the range normally ordered for water and air coolers; other diameters and walls are produced to the same specification.
| Outside diameter | Common wall thickness | Typical use |
|---|---|---|
| 19.05 mm, 3/4 in. | 0.89 mm and 1.24 mm | Shell and tube water coolers, air coolers |
| 25.40 mm, 1 in. | 0.89 mm to 1.65 mm | Surface condensers, evaporators |
| Other diameters to 79.4 mm, 3-1/8 in. | as specified on the order | Power and process exchangers |
Straight lengths are cut to the ordered length or to a manufacturing length of up to about 6 m, with the ends squared and deburred. U-bent tube is bent to the required centre-line radius with the bend portion annealed, and is normally supplied with the legs trimmed to the drawing.
Applications in Water and Air Cooler Condensers
Surface condensers and dump condensers in thermal power and industrial steam systems.
Shell and tube water coolers, oil coolers and after-coolers on engines and compressors.
Air cooler and air-conditioning condensers where fresh or brackish cooling water is used.
Evaporators, desalination preheaters and marine auxiliary exchangers.
Feedwater heaters and general heat-transfer circuits where seawater or brackish water is the cooling medium.
The alloy is selected primarily for its tolerance of flowing water. Where chloride levels are very high, or where ammonia or sulphide contamination is expected, aluminium brass or copper-nickel grades are preferred instead, and the tube material should be confirmed against the water chemistry of the specific circuit.
Selection, Installation and Corrosion Control
Corrosion failures in admiralty brass tube are usually caused by conditions rather than by the alloy: excessive water velocity, entrained air bubbles, deposits that create differential aeration cells, or residual stresses from bending. Practical measures that keep the tube within its design envelope are given below.
Keep cooling-water velocity within the range recommended for the alloy, generally about 1.0-2.0 m/s for clean seawater, and control the velocity at tube inlets with ferrules or with an epoxy coating at the inlet end.
Eliminate air pockets and vent the circuit, because entrained gas promotes impingement attack at the tube inlet.
Relieve residual stress on U-bends and on expanded tube ends by a suitable anneal, and avoid cold working after the final anneal.
Maintain water treatment: control chlorides, pH, suspended solids and dissolved oxygen, and prevent ammonia from reaching the tube side.
Clean on a schedule by brushing or by chemical methods approved for copper alloys; avoid wire tools and acid concentrations that attack the protective film.
Roller-expand tubes into the tube sheet to the recommended expansion percentage, and confirm joint tightness before service.
During storage, tubes should be kept dry and protected from chlorides, because condensation between stacked tubes can start pitting before the exchanger is assembled.
FAQ
Q: What is the difference between admiralty brass C44300 and C44300B?
Both designations refer to the same UNS C44300 composition; the letter suffix is a supplier product or order code. When comparing offers, request the chemical analysis and the ASTM B111/B111M temper, which are the values that actually govern performance.
Q: Is admiralty brass tube suitable for seawater?
Yes, for clean and moderately polluted seawater within the recommended velocity range. The tin and arsenic additions specifically protect against impingement attack and dezincification. For heavily polluted water, high suspended solids or ammonia-bearing condensate, aluminium brass or copper-nickel tube is normally a better choice.
Q: Which temper should be ordered for a condenser?
Annealed tube is standard, because it can be rolled into the tube sheet and U-bent without cracking. Hard-drawn tube is ordered only for straight tube where no forming is required.
Q: How is tube quality verified before shipment?
By tension, expansion and, when specified, flattening or bending tests, together with eddy-current examination to ASTM E243 and a hydrostatic or pneumatic pressure test. The mill certificate reports the chemical analysis and the mechanical results for the heat and lot.
Q: What wall thickness is normally used?
Wall thickness follows the exchanger design pressure and the allowance for corrosion. Common condenser walls are 0.89 mm and 1.24 mm, and thicker walls are used where water quality is aggressive or where the tube is expected to be re-rolled at the tube sheet.
Q: Can admiralty brass be welded?
The alloy is normally joined by expansion into tube sheets or by brazing rather than fusion welding. Where welding is unavoidable, a copper-based filler and a qualified procedure are used, and the joint is stress relieved to avoid service cracking.