What C10100 Oxygen-Free Electronic Copper Is
C10100, also written OFE copper, is a high-purity copper grade in which the residual oxygen content is deliberately kept at or below 0.0005 %. Ordinary tough-pitch copper contains oxygen as cuprous oxide particles that are harmless in plumbing but harmful in a vacuum or high-frequency environment, because the oxide breaks down when the metal is heated in a reducing atmosphere and the resulting steam causes internal porosity and cracking. Removing the oxygen eliminates that mechanism, which is why oxygen-free copper is specified for electron devices, vacuum components and superconducting magnet stabilisers.
The related grade C10200, oxygen-free copper without the electronic designation, is used where the very tight residual-resistance requirements of C10100 are not needed. C11000 electrolytic tough pitch copper remains the low-cost alternative for busbars, wiring and general electrical work.
Chemical Composition and Purity Control
| Element | Limit | Function |
|---|---|---|
| Cu | ≥ 99.99 % | Balance, principal element |
| O | ≤ 0.0005 % | The key control item; prevents hydrogen embrittlement |
| P | ≤ 0.0003 % | Kept low because phosphorus sharply reduces conductivity |
| Other elements | individually limited, total ≤ 0.01 % by difference | Silver, sulphur, selenium and other residuals are restricted to protect conductivity |
Note that 99.99 % minimum copper means the sum of everything else cannot exceed 0.01 %. The individual limits for residual elements are listed in ASTM B170 for the wrought grade and are repeated in the tube product standard ASTM B68/B68M, which covers seamless copper tube intended for general engineering and electronic duty.
Physical, Electrical and Thermal Properties
| Property | Typical value |
|---|---|
| Density | 8.94 g/cm³ |
| Melting point | 1083 °C |
| Electrical conductivity at 20 °C | ≥ 101 % IACS |
| Thermal conductivity | approximately 391 W/(m·K) |
| Coefficient of thermal expansion | 17.0 × 10-6/K over 20–300 °C |
The conductivity figure is the reason this grade exists. A tube that carries a high-frequency signal is judged by its surface losses, and a tube that forms the wall of a vacuum chamber must not release gas. Both requirements are met by a metal that is nearly free of dissolved oxygen and of electrically active impurities.
Mechanical Properties by Temper
| Temper | Tensile strength (MPa) | Yield strength (MPa) | Elongation (%) | Typical use |
|---|---|---|---|---|
| Annealed (O60) | 220–270 | about 70 | ≥ 45 | Bent and coiled tube, waveguides, flexible connections |
| Hard drawn (H) | 350–400 | about 330 | ≥ 4 | Straight runs, structural or self-supporting tube |
These are typical values for the grade rather than a substitute for the purchase specification. The order should state the temper, the outside diameter and wall thickness, and the product standard, because the same outside diameter is produced in several wall thicknesses.
Applications in Electronics and Electrical Engineering
High-frequency coaxial cable conductors, rigid coaxial lines and waveguides, where surface conductivity controls attenuation.
Vacuum tubes, magnetrons, klystrons and travelling-wave tubes, where the metal must be brazed and then evacuated without releasing gas.
Transistor components, lead frames and heat spreaders that combine electrical conduction with heat removal.
Stabilisers and cryogenic components for superconducting magnet systems, including liquid helium-cooled assemblies.
Power transmission busbar and heavy current connections where conductivity is valued above cost.
Vacuum chambers for particle accelerators, sputtering targets and critical parts of wafer fabrication equipment.
Fabrication, Brazing and Handling
Oxygen-free tube is normally joined by brazing in a controlled atmosphere or in vacuum. Because there is no oxide present to decompose, the joint may be made in dry hydrogen without the risk of steam formation inside the wall. Parts should be degreased and handled with clean gloves; fingerprints and chloride residues cause the surface staining that later shows up as a defect after annealing. Bending, flaring and swaging practices are the same as for other seamless copper tube, but hard drawn tube should be annealed locally before severe forming. Annealing is carried out in a protective or reducing atmosphere to keep the surface bright.
FAQ
Q: What does OFE mean in C10100?
OFE stands for oxygen-free electronic. It indicates copper refined to a minimum of 99.99 % copper with oxygen held at or below 0.0005 %, which gives the highest conductivity of the wrought copper grades.
Q: Why is oxygen a problem in copper tube?
Oxygen is present as cuprous oxide particles. When the metal is heated in a reducing atmosphere such as hydrogen, the oxide reacts and generates steam inside the metal, which causes porosity and cracking known as hydrogen embrittlement.
Q: Is C10100 tube the same as C11000 tube?
No. C11000 is electrolytic tough pitch copper containing oxygen and offering about 100 % IACS. C10100 is oxygen-free with at least 101 % IACS and is intended for vacuum, electronic and high-frequency service.
Q: Which standard covers this tube?
ASTM B68/B68M covers seamless copper tube, while ASTM B170 defines the oxygen-free electronic copper grade itself. Dimensional and tolerance data are given in the tube standard.
Q: Can C10100 tube be welded?
It can be welded, but brazing in vacuum or in a reducing atmosphere is the usual production route because it produces a clean joint with the least risk of contamination of the high-purity metal.
Q: How is the finished tube inspected?
Eddy-current testing is the standard non-destructive method for seamless tube, supported by dimensional checks and by chemical analysis of the heat to confirm the conductivity and purity limits.