What C72200 Nickel-White Copper Is
C72200 is a copper-nickel alloy in the UNS numbering system, often described as chromium-modified 85/15 cupronickel because it contains nominally 15 % nickel together with a deliberate chromium addition. In the trade the alloy is also called nickel-white copper. It was developed for condenser and heat exchanger tubing where the cooling water is seawater or brackish water and flow velocities are high enough to attack conventional cupronickel or aluminium brass tubes.
The distinguishing feature of C72200 is the chromium content. Chromium in this alloy improves resistance to impingement attack and erosion corrosion, so the tube can tolerate higher seawater velocities than an unmodified copper-nickel grade while still forming the thin, stable corrosion product film that protects copper-nickel alloys in clean seawater.
Chemical Composition
| Element | Content | Function |
|---|---|---|
| Nickel, including cobalt | 15.0 % to 18.0 % | Principal alloying addition; gives strength and seawater corrosion resistance |
| Chromium | 0.30 % to 0.70 % | Improves resistance to impingement and erosion corrosion at higher flow velocities |
| Iron | 0.50 % to 1.00 % | Improves resistance to flowing seawater attack |
| Manganese | 0.50 % to 1.00 % | Deoxidizes the melt, assists castability and hot workability |
| Titanium | 0.50 % maximum | Controlled residual from deoxidation practice |
| Copper | Remainder | Base of the alloy |
| Other elements | Limited | Impurity limits applied to protect weldability and formability |
Composition limits for the alloy in tube form are published in ASTM B111, and plate, sheet and strip of the same grade are covered by ASTM B122. Cobalt is counted with the nickel when the analysis is checked, which is standard practice for copper-nickel alloys, and iron plus manganese together define much of the seawater performance of the material.
Mechanical Properties and Tempers
The mechanical properties of C72200 depend on the temper in which the tube or sheet is supplied, exactly as with other wrought copper alloys. Soft annealed temper is used where the tube has to be bent or expanded, and cold worked tempers raise strength and hardness at the cost of ductility. For tube supplied under ASTM B111, tensile strength, yield strength measured at 0.5 % extension under load, and elongation are specified in the standard for the ordered temper, and the mill certificate reports the actual values for the lot.
A practical consequence is that the buyer should specify the temper and the product standard rather than quoting a single tensile strength figure. Two tubes of identical chemistry can differ substantially in strength simply because one was annealed and the other was drawn to a cold worked temper.
| Property | Behaviour of C72200 |
|---|---|
| Tensile strength | Tabulated minimum for the ordered temper in ASTM B111; cold working raises it, annealing lowers it |
| Yield strength | Measured at 0.5 % extension under load and specified with the temper; cold worked tube is markedly stronger than annealed tube |
| Elongation | Highest in the annealed temper, which is why annealed tube is used for bending and expanding |
| Hardness | Increases with cold work; used as a shop floor check that the temper is correct |
| Modulus of elasticity | Approximately 130 GPa, typical of the copper-nickel family |
| Density | About 8.9 g/cm³ |
| Crystal structure | Face-centred cubic, giving good ductility |
Corrosion and Physical Behaviour
In clean, aerated seawater C72200 forms a protective corrosion product film that keeps the corrosion rate low and uniform. The chromium addition extends the velocity range over which the film survives, which is the reason the alloy is used in condensers where tube velocities are pushed higher to improve heat transfer. Copper-nickel alloys are also resistant to chloride stress corrosion cracking, which is an advantage over the austenitic stainless steels in warm chloride environments.
Two limitations should be understood. Copper-nickel alloys can suffer stress corrosion cracking in ammoniacal environments, so polluted seawater, condensate from ammonia bearing systems and ammonia vapour around tube sheets all deserve attention. And the alloy is not immune to under-deposit corrosion; scale, sludge or biological growth on the water side starves the surface of oxygen and creates the local conditions for pitting beneath the deposit.
Electrical conductivity is a small fraction of that of pure copper, and thermal conductivity, while lower than pure copper, is more than adequate for seawater cooled heat transfer duty. C72200 is chosen for corrosion performance under flow, not for conductivity.
Heat Treatment and Fabrication
C72200 is normally supplied in the annealed condition for tube applications. Annealing and stress relief treatments must be carried out at temperatures that soften the material without coarsening the structure excessively, and the schedule should be specified on the order rather than improvised in the workshop. Quoting a heat treatment temperature that is nonsense is a reliable way to destroy a batch of tube, so the temperature range should always come from the material supplier and be recorded in the process sheet.
Cold working is excellent, so tubes can be bent and rolled into tube sheets without cracking when the correct temper is supplied.
Hot working is carried out in a temperature range below the melting point of the alloy and above the temperature at which the material becomes brittle.
Annealing is used between cold forming operations when a large total reduction is required.
Welding and brazing are practicable with fillers matched to the alloy; the chromium and titanium additions mean that heat input and interpass temperature should be controlled.
Stress relief after heavy forming is good practice for components that will see ammoniacal service.
Where C72200 Is Used
Condenser and heat exchanger tubes in power stations, ships and desalination plants using seawater
Tube plates and water boxes in seawater cooled equipment
Piping and fittings in marine and offshore systems
Components exposed to high velocity seawater where erosion corrosion is the limiting factor
Inspection Points and Common Pitfalls
Confirm the grade by certificate, checking nickel with cobalt, chromium, iron and manganese against the specification limits.
Verify the temper and the corresponding tensile, yield and elongation values for the lot.
Eddy-current test the tube for wall defects before installation and keep the record as a baseline.
Check grain size and surface condition, since both affect bending and rolling performance.
Keep the tubes dry and free of chloride contamination before installation.
The recurring pitfall is to treat all cupronickels as one material. Unmodified copper-nickel and the chromium-modified grade differ in the velocity range they tolerate, and C72200 should not be ordered simply because a quotation mentioned cupronickel tube. Name the UNS grade and the standard on the order, and ask for the analysis and the mechanical test results on the certificate.
FAQ
Q: What is C72200 nickel-white copper?
It is a chromium-modified copper-nickel alloy containing nominally 15 % nickel, used mainly for condenser and heat exchanger tubes in seawater service.
Q: How does C72200 differ from ordinary cupronickel?
The chromium addition, in the range of 0.30 % to 0.70 %, improves resistance to impingement and erosion corrosion so that the tube tolerates higher seawater velocities.
Q: Which standard covers C72200 tube?
Seamless tube is specified in ASTM B111, and plate, sheet and strip of the same grade in ASTM B122.
Q: What temper is used for condenser tubes?
Soft annealed tube is normal, because it must be bent and expanded into the tube sheet without cracking. Cold worked tempers are used for other product forms.
Q: Can C72200 be welded?
Yes, with fillers matched to the alloy and controlled heat input. As with all copper-nickel alloys, cleanliness of the joint area and control of interpass temperature are essential.
Q: What limits the service life of C72200 tubes?
Polluted or ammoniacal water, deposits that cause under-deposit pitting, and excessive flow velocity. In clean seawater with correct water treatment, the alloy gives very long service.