What H96 Brass Is
H96 is a wrought copper-zinc brass with the highest copper content of the common H-series grades, containing nominally 96 % copper with zinc as the balance. Its very low zinc level keeps it in the single-phase alpha region, where the alloy retains the warm colour, high thermal and electrical conductivity and excellent formability of copper while gaining useful strength and improved resistance to tarnishing. In Chinese practice the grade belongs to the wrought copper alloy system described by GB/T 5231, and in international ordering it is broadly comparable with the high-copper gilding brass grades such as UNS C21000.
The commercial significance of the grade is that it sits between pure copper and the lower brasses. It works almost as easily as copper in cold forming, brazes and solders well, resists atmospheric and freshwater attack, and costs less than pure copper, but it does not offer conductor-grade conductivity. That combination is what makes it a standard choice for cooling equipment components, electrical hardware and precision pressed parts.
Chemical Composition and Designation of H96
H96 is defined by its copper content and by tight limits on the residual elements that would otherwise damage conductivity and formability. Zinc makes up the balance, and the residuals are controlled as follows:
Copper: nominal 96 %, which gives the grade its designation under the H plus copper content rule.
Zinc: balance, remaining in the single-phase alpha range.
Lead: 0.03 % maximum, limited because lead forms low-melting grain boundary films that embrittle hot working.
Iron: 0.10 % maximum, controlled because iron reduces conductivity and can form hard particles in the matrix.
Phosphorus: 0.01 % maximum, since even small phosphorus additions sharply reduce electrical conductivity.
Total impurities: 0.2 % maximum, which is what keeps the high conductivity and ductility of the grade predictable.
Because the composition limits, temper designations and permissible tolerances are set by the applicable product standard rather than by the designation alone, an order for H96 should always name the standard and the product form, for example strip to GB/T 2059 or sheet, strip and plate to ASTM B36, together with the required temper and dimensions.
Physical and Mechanical Properties
| Property | Typical value for H96 | Remark |
|---|---|---|
| Density | About 8.85 g/cm³ | Slightly below pure copper, consistent with the 4 % zinc addition |
| Melting range | About 1065 °C | Slightly lower than pure copper |
| Electrical conductivity | Well below pure copper | Conductivity falls steeply as zinc is added, so H96 is a working material, not a conductor material |
| Thermal conductivity | High, in line with its copper content | Supports heat transfer in cooling and electrical hardware |
| Coefficient of thermal expansion | About 18.5 × 10⁻⁶/K between 20 and 300 °C | Relevant to brazed and soldered assemblies |
| Tensile strength | About 205 to 320 MPa depending on temper | Higher than soft pure copper, the lowest range among the common brasses |
| Elongation | From a few per cent in the hard temper up to about 45 % in the annealed temper | Indicates the wide forming window of the grade |
| Hardness | About 45 to 105 HV depending on temper | Cold work raises hardness and strength together |
The property pattern is characteristic of a high-copper brass: strength increases and ductility decreases with cold work, and an anneal restores ductility at the cost of the strength gained. That is why the temper, not just the grade, determines what the delivered strip or tube will do in a press or a bending die.
Processing, Annealing and Joining Notes
H96 responds well to cold working, which is how most of it is processed into strip, sheet, tube and pressed parts. Between cold operations an anneal at around 540 to 600 °C relieves the internal stress introduced by deformation and restores elongation; the same treatment is used to stress relieve finished parts where stress corrosion cracking is a concern. Hot working is carried out in the recommended range of roughly 640 to 850 °C, above which grain growth and surface oxidation become significant and below which the alloy loses ductility.
For joining, H96 is readily soldered and brazed, and it can be welded with appropriate processes and filler metals. Two precautions matter. First, residual stress left in a cold-formed part should be relieved before the part enters an environment containing ammonia or amines, because stressed high-copper brasses are susceptible to stress corrosion cracking; the ammonia vapour test used for heat exchanger tube under ASTM B111 exists for exactly this reason. Second, because H96 already contains zinc, the zinc loss and tarnish that affect lower brasses at high temperature are less severe, but brazing should still be done with controlled atmospheres or suitable flux to avoid oxidation of the joint area.
Applications of H96 Brass
The combination of high workability, good thermal performance and corrosion resistance in atmospheric and freshwater conditions determines where the grade is used:
Cooling equipment: condenser and radiator components, cooling coils and heat transfer parts, where corrosion resistance and thermal conductivity both matter.
Electrical and electronic hardware: contact plates, conductive terminals, connector shells and shielding parts, where formability and stable contact behaviour are needed rather than conductor-grade conductivity.
Precision mechanical parts: bushings, gears, valve components and small stampings produced by cold pressing, deep drawing or machining.
Decorative and architectural parts: high-copper brasses such as H96 and H90 have the golden colour and tarnish resistance expected of architectural trim, plaques and hardware.
Brazing and soldering assemblies: the grade's clean, oxide-free brazing behaviour makes it a carrier material in composite and heat transfer assemblies.
Common Misconceptions and Grade Selection
Two misconceptions cause most grade selection errors. The first is the belief that a high-copper brass conducts like pure copper. In binary copper-zinc alloys, conductivity falls steeply as zinc is added, and even 4 to 5 % zinc is enough to pull conductivity far below the conductor-grade level; H96 therefore has no role in busbars, windings or cable, which belong to the C10100, C11000 and silver-bearing copper grades. The correct basis for selecting H96 is formability, colour, thermal performance and dependable corrosion behaviour at a lower cost than pure copper.
The second misconception is that the designation alone specifies the delivered product. H96 strip can be delivered annealed, quarter hard or hard, and each temper has different strength and elongation; a buyer who specifies only the grade can receive a material that will not form in the intended die or that has insufficient stiffness for the finished part. The order should state the grade, the standard, the temper, the dimensions and the inspection requirements, and for critical applications should ask for the chemical analysis and the mechanical test results to be certified.
FAQ
Q: Is H96 brass the same as pure copper?
No. H96 contains nominally 96 % copper with zinc as the balance, so it is an alloy rather than pure copper. It has higher strength and better tarnish resistance than soft copper but clearly lower electrical conductivity, and it is not acceptable for conductor applications.
Q: What is the electrical conductivity of H96 brass?
It is substantially lower than that of pure copper. In the copper-zinc system, conductivity falls steeply as zinc is added, so the 4 % zinc in H96 is already enough to remove it from conductor duty. Orders should specify conductivity only where the application genuinely needs it, and should then state the test method and acceptance limit.
Q: What does the number 96 mean in H96?
Under the Chinese designation system for wrought copper alloys, the letter H denotes brass and the number gives the nominal copper mass fraction, so H96 contains about 96 % copper and about 4 % zinc, with strictly limited residuals of lead, iron and phosphorus.
Q: Why is the lead content of H96 limited to 0.03 %?
Lead forms low-melting films along the grain boundaries and causes hot shortness during rolling and drawing. Keeping lead, phosphorus, iron and total impurities low preserves the ductility and conductivity that make the grade useful in deep drawing and pressing.
Q: At what temperature is H96 annealed?
Annealing to relieve internal stress and restore ductility is normally carried out around 540 to 600 °C. Hot working is performed in roughly the 640 to 850 °C range, and the exact schedule depends on the product form, the amount of prior cold work and the required final temper.
Q: Can H96 be used in seawater?
H96 resists the atmosphere and fresh water well and is used in cooling and radiator components, but it is not an alloy designed for continuous seawater service. Marine and condenser duties belong to the copper-nickel and admiralty brass families, which contain nickel, tin or aluminium additions that form a stable protective film in chloride environments.