What the C71500 Grade Is
C71500 is the UNS designation for 70/30 copper-nickel, a copper base with 29-33 % nickel and controlled iron and manganese. It is a single-phase alloy with a face-centred cubic structure and it is essentially non-magnetic, which is one reason it is used in instrument and marine components as well as for heat transfer tube. Its mechanical behaviour follows the familiar copper-alloy pattern: strength comes from solid-solution hardening by nickel plus whatever cold work the temper imposes, and ductility is recovered by annealing.
Mechanical requirements are therefore never quoted for the alloy alone. They are quoted for a specified product form and temper, because an annealed seamless tube to ASTM B111 and a hard-drawn rod to ASTM B151 of the same alloy have very different properties.
Tensile, Yield and Elongation Requirements
| Condition | Tensile strength | 0.5 % offset yield strength | Elongation in 50 mm |
|---|---|---|---|
| Annealed tube, ASTM B111 (O61) | 380 MPa (55 ksi) minimum | 140 MPa (20 ksi) minimum | 30 % minimum |
| Light drawn tube | Higher minima than annealed, tabulated in the specification | Higher than annealed, tabulated in the specification | Lower than annealed, tabulated in the specification |
| Hard drawn tube | Highest tensile minima of the tube tempers | Highest yield minima of the tube tempers | Lowest elongation of the tube tempers |
| Typical annealed values in production | 380 - 450 MPa | 140 - 200 MPa | 30 - 40 % |
Two conventions matter when reading a cupronickel test certificate. The first is that the yield strength is quoted at 0.5 % offset for copper-nickel tube rather than at the 0.2 % offset used for steel. The second is that tensile and yield minima for annealed tube sit well below the values obtained in routine production, so a certificate showing comfortable margins is normal and is not by itself evidence of an off-standard heat.
Hardness and Elastic Constants
Typical hardness for annealed 70/30 tube lies in the range of about 80-120 HB, rising as the tube is cold drawn and reducing again after annealing. Hardness is a useful shop-floor indicator of temper consistency, but it is not a substitute for the tensile test when compliance has to be demonstrated.
| Property | Typical value |
|---|---|
| Elastic modulus | About 150 GPa |
| Shear modulus | About 52 GPa |
| Poisson ratio | About 0.34 |
| Density | 8.94 g/cm³ |
| Melting range | Approximately 1170 - 1240 degrees C |
| Thermal conductivity at 20 degrees C | About 29 W/(m·K) |
| Electrical conductivity | Approximately 4.6 % IACS |
How Temper and Temperature Change the Properties
Cold reduction is the only practical way to raise the strength of a cupronickel tube after it has been annealed, and the trade is direct: every increment of drawn temper raises tensile and yield strength and lowers elongation. A tube intended for roller expansion into a tube sheet is normally annealed, because expansion requires ductility; a tube intended to resist wear in a slurry duty may be supplied in a drawn temper where the higher surface hardness is worth the loss of formability. Where cold forming has been carried out, a stress relief anneal restores ductility and removes the residual stresses that would otherwise make the component sensitive to stress corrosion cracking.
At elevated temperature, tensile and yield strength fall steadily and creep becomes the design consideration; 70/30 copper-nickel is commonly used in continuous service at temperatures up to about 400 degrees C, with properties reducing as temperature rises. At low temperature the alloy retains good toughness and is used for cryogenic tube, since it has no ductile-to-brittle transition of the kind found in ferritic steels.
Testing and Acceptance Evidence
Mechanical compliance is demonstrated by tension testing, carried out for copper alloys in accordance with ASTM E8 and E8M, with hardness measured by the Brinell method under ASTM E10 when a hardness figure is required. Tube to ASTM B111 is additionally subjected to flattening and expansion tests, which are forming tests rather than property tests and are used to demonstrate that the tube will survive the mechanical operations of bundle assembly. Dimensional checks, a hydrostatic or pneumatic pressure test as ordered, and eddy-current examination to Practice E243 complete the usual acceptance package.
A purchaser reviewing a mill certificate should check that the alloy is identified as UNS C71500, that the temper matches the order, that tensile, yield and elongation values are on the correct side of the specified minima, that the yield value is stated at 0.5 % offset, and that the mechanical results correspond to the same heat and lot as the dimensional and non-destructive results.
FAQ
Q: What is the tensile strength of C71500?
Annealed tube to ASTM B111 must reach at least 380 MPa (55 ksi); typical production values are 380-450 MPa, and cold-drawn tempers are specified with higher minima.
Q: What yield strength should be expected?
The specification minimum for annealed tube is 140 MPa (20 ksi) at 0.5 % offset, with typical production values in the range 140-200 MPa. Copper-nickel tube yields are quoted at 0.5 % offset rather than 0.2 %.
Q: How hard is C71500?
Annealed 70/30 tube is typically about 80-120 HB. Hardness rises with cold reduction and falls again after annealing, so it is a useful shop indicator of temper rather than a substitute for tension testing.
Q: What is the elastic modulus of the alloy?
The elastic modulus is about 150 GPa with a shear modulus near 52 GPa and a Poisson ratio of about 0.34.
Q: How hot can C71500 be used?
Continuous service at up to approximately 400 degrees C is normal for the 70/30 grade, but tensile and yield strength decrease as temperature rises and creep becomes the controlling design factor at the upper end of that range.
Q: Which tests demonstrate mechanical compliance?
Tension testing to ASTM E8 and E8M provides the tensile, yield and elongation values, hardness when required is measured by the Brinell method to ASTM E10, and tube to ASTM B111 is additionally given flattening and expansion tests.