Dec 29, 2025 Leave a message

C26000 Yellow Brass: Composition, Properties and Applications

C26000 yellow brass is the most ductile member of the yellow brass family and the grade most often quoted when a component has to be formed aggressively and then hold its shape. Designers meet the alloy in ammunition cases, architectural hardware, plumbing components and electrical parts, yet the reasons it behaves well in those very different duties all come back to the same balance of copper and zinc.

Why the Alloy Is Called Yellow Brass

Yellow brass is the traditional name for copper-zinc alloys in which zinc is the main alloying addition. As zinc rises, colour shifts from the reddish tone of copper through gold to a paler yellow, strength increases and ductility falls. C26000 sits at the sweet spot: a nominal 70 % copper and 30 % zinc content gives the bright yellow-gold appearance that decorative hardware expects while keeping a single-phase alpha structure that stays formable at room temperature.

Because the structure is entirely alpha, C26000 is not hot-short and does not need the hot-working precautions that apply to two-phase brasses. It hardens steadily during cold work, which lets a stamping shop plan a predictable annealing schedule instead of improvising around cracking.

Composition and Governing Standards

Lead is held at 0.07 % maximum, so C26000 belongs to the low-lead brass group. Iron is limited to 0.05 % because hard iron particles reduce elongation, and total unspecified impurities are capped at 0.15 %. Each product form is controlled by its own standard, and the applicable standard should always be stated on the order.

Product form Standard Typical use of the form
Sheet, strip and plate ASTM B19, ASTM B36 Deep-drawn cups, hardware, heat exchanger shells
Wire ASTM B134 Fasteners, rivets, eyelets, woven mesh
Seamless tube ASTM B135 Small-diameter tube, ferrules, instrument lines
Strip for heat exchangers ASTM B569 Finned tube and radiator strip
Welding rod ASTM B587 Brazing and welding consumables

Mechanical and physical property requirements follow the temper ordered under the ASTM B601 temper designation system, and the exact tensile and elongation limits for a given temper line must be taken from the standard rather than assumed.

Physical and Mechanical Behaviour

Property Value
Density 8.53 g/cm³ (0.308 lb/in³)
Melting range 915 – 955 °C
Electrical conductivity (annealed) about 28 % IACS
Thermal conductivity about 120 W/(m·K)
Modulus of elasticity 110 GPa
Typical tempers O60, H01, H02, H04, H06, H08

Strength and hardness climb quickly with cold reduction while elongation drops, which is why a part with a difficult forming sequence is specified in soft temper and a spring-contact part is specified in a spring temper. Thermal and electrical conductivity are adequate for current-carrying hardware, and the alloy remains non-magnetic throughout.

Corrosion Behaviour

C26000 performs well in fresh water, sea air, industrial atmospheres and most neutral or mildly alkaline media. Three families of media must be avoided or controlled:

Ammonia and ammonium compounds: these attack brass and, in the presence of residual stress, trigger stress corrosion cracking. Stress-relief annealing at 250 – 325 °C is the standard countermeasure.

Acids: acetic, hydrochloric and nitric acid solutions corrode the alloy rapidly and are outside its service envelope.

Aggressive chlorides: long exposure to high-chloride water can promote selective attack on high-zinc brasses, so water chemistry is reviewed before the grade is released for a piping duty.

Typical Applications

Sector Components
Defence and sporting Ammunition casings and drawn cases
Building products Locks, hinges, decorative hardware, bathroom fixtures
Plumbing Fittings, valves bodies, ferrules, fasteners
Electrical Terminals, contact springs, lamp fittings, eyelets
Heat transfer Radiator strip, shell plates, tube sheets

FAQ

Q: What makes C26000 different from other yellow brasses?
It retains a fully alpha structure at room temperature, so it is more ductile and more suitable for severe cold forming than brasses with higher zinc content.

Q: Is C26000 suitable for potable water fittings?
Its lead content is restricted to 0.07 % maximum, but the finished part must still satisfy the lead-leaching rules of the destination market before release.

Q: How is C26000 ordered?
Order by UNS number, product form, temper designation, dimensions, edge condition and the applicable ASTM standard, then add any grain size requirement separately.

Q: Does C26000 lose conductivity when it is cold worked?
Cold work raises strength and lowers electrical conductivity slightly; soft-temper material is selected when the conductivity value matters.

Q: What causes season cracking in yellow brass?
Ammonia or ammonium exposure acting on residual stress from cold work; stress-relief annealing removes the residual stress and the risk.

Q: Can C26000 parts be plated?
Yes. The alloy takes nickel, tin and chromium plating well after standard cleaning and activation, and plating is common on decorative hardware.

Send Inquiry

whatsapp

Phone

E-mail

Inquiry