Material Identification
C11000 is the UNS designation for electrolytic tough pitch copper, frequently abbreviated ETP copper. It is the workhorse high-conductivity copper of the electrical industry, combining full conductivity with good formability at a lower cost than the oxygen-free grades. The table below lists the designations used across the main standards systems.
| System | Code | Standard reference |
|---|---|---|
| UNS designation | C11000 | ASTM B152, ASTM B124, ASTM B187 |
| European designation | CW004A | EN 1412 numbering system |
| Japanese designation | C1100 | JIS H3100 |
| ISO designation | Cu-ETP | International designation system |
Chemical Composition
The specification is deliberately simple: the material is copper with a controlled oxygen addition that improves fluidity during casting and reduces the risk of porosity in the cast bar. Silver is counted with the copper content and is not an intentional addition.
| Element | Limit | Typical | Function |
|---|---|---|---|
| Copper plus silver | 99.90% minimum | 99.95% | Primary constituent |
| Oxygen | 0.040% maximum | 0.02-0.04% | Present as cuprous oxide; improves castability |
| Silver | 0.030% maximum | about 0.015% | Counted within the copper total |
| Lead | 0.005% maximum | about 0.002% | Impurity control |
| Iron | 0.005% maximum | about 0.002% | Impurity control |
| Tin | 0.002% maximum | below 0.001% | Impurity control |
| Zinc | 0.002% maximum | below 0.001% | Impurity control |
| Total other impurities | 0.050% maximum | about 0.020% | Excluding oxygen |
Physical and Electrical Properties at 20 C
| Property | Metric | Imperial | Test method |
|---|---|---|---|
| Electrical conductivity | 58 MS/m or higher (100% IACS) | 100% IACS or higher | ASTM E1004 |
| Electrical resistivity | 1.724 micro-ohm-cm | 6.79 micro-ohm-in | ASTM B193 |
| Temperature coefficient of resistance | 0.00393 per C | 0.00218 per F | Calculated from resistivity data |
| Thermal conductivity | 390 W/(m K) | 270 BTU-ft/(h-ft²-F) | ASTM E1461 |
| Specific heat capacity | 0.385 J/(g K) | 0.092 BTU/(lb F) | Calorimetry |
| Thermal expansion, 20-300 C | 16.5 × 10-6 per C | 9.2 × 10-6 per F | ASTM E228 |
| Density | 8.94 g/cm³ | 0.323 lb/in³ | Gravimetric |
| Melting point | 1083 C | 1981 F | Pure metal constant |
| Elastic modulus | 117 GPa | 17000 ksi | ASTM E111 |
| Poisson ratio | 0.34 | 0.34 | Reference value |
Mechanical Properties and Tempers
In the annealed condition the material is soft and highly ductile, which suits the forming operations that dominate busbar and heat exchanger production. Cold working raises strength and hardness progressively, and the limits listed below are representative of commercial supply rather than a guarantee for every gauge.
| Condition | Tensile strength | Yield strength, 0.2% | Elongation | Hardness |
|---|---|---|---|---|
| Annealed, O60/O61 | 210-250 MPa | 70-100 MPa | 45-55% | 45-65 HRB |
| H02 half hard | about 300 MPa | about 200 MPa | about 25% | about 70 HRB |
| H04 hard | about 350 MPa | about 280 MPa | about 10% | about 85 HRB |
| H08 spring | about 400 MPa | about 320 MPa | about 5% | about 95 HRB |
Fatigue behaviour in the annealed condition is moderate, with an endurance limit of roughly 90 MPa under rotating beam loading at 10 to the seventh cycles. Fatigue strength improves with cold work but elongation falls, so the temper should be chosen against the actual load cycle rather than on strength alone.
Fabrication, Corrosion and Applications
| Operation | Suitability | Notes |
|---|---|---|
| Cold drawing and deep drawing | Excellent | Annealed temper preferred |
| Bending | Excellent | Minimum radius close to one thickness when annealed |
| Stamping and blanking | Excellent | Clean sheared edges with correct clearance |
| Hot working | Good | Practised between roughly 700 C and 900 C |
| Soft soldering | Excellent | Rosin-based flux gives reliable joints |
| Silver brazing | Excellent | Widely used in heat exchanger manufacture |
| TIG or MIG welding | Limited | Porosity must be controlled |
| Machining | Good | Carbide tooling with flood coolant |
Corrosion performance follows that of pure copper. In urban and industrial atmospheres and in fresh water the metal forms a protective oxide and corrodes at rates below 0.01 mm per year, and it is suitable for potable water service. In seawater the general performance is acceptable at low flow velocities, but a copper-nickel grade is preferred where velocity exceeds roughly 2 m per second. In reducing atmospheres, particularly hydrogen-bearing ones, C11000 is unsuitable because the cuprous oxide it contains can react with hydrogen and cause embrittlement.
Applications follow directly from this profile: busbars and switchgear contacts, transformer windings, printed circuit and connector stock, heat exchanger tubes and coils, refrigeration lines, plumbing and architectural elements, automotive radiators and brake lines, and marine piping systems. Product forms include tube and pipe from roughly 3 mm to 152 mm outside diameter, sheet from about 0.15 mm to 4.8 mm and plate above that, bar from 3 mm to 150 mm diameter, and wire from 0.25 mm to 12.7 mm diameter.
Quality control for the grade normally combines chemical analysis of copper and oxygen on each heat, tensile and hardness testing per lot, eddy current conductivity testing of the finished product, dimensional checks by micrometre or gauge, and surface examination by eddy current or visual inspection where the application demands it.
FAQ
Q: What does ETP copper mean?
ETP stands for electrolytic tough pitch; the copper is refined electrolytically and then cast with a controlled oxygen content that improves casting behaviour.
Q: Is C11000 the same as C10200?
No. Both are high-conductivity coppers, but C11000 contains up to 0.040% oxygen while C10200 is oxygen-free at 0.001% maximum and is used where reducing atmospheres or vacuum service are involved.
Q: Can C11000 be used in hydrogen atmospheres?
It should not be. The cuprous oxide present can react with hydrogen at elevated temperature and cause internal cracking, so an oxygen-free grade is required instead.
Q: What is the conductivity of C11000?
58 MS/m or better, equivalent to 100% IACS or slightly above, measured by eddy current testing per ASTM E1004.
Q: Which standards apply to the different product forms?
ASTM B152 covers sheet, strip, plate and rolled bar, B124 covers rod and bar, B187 covers busbar, and tube products are covered by the relevant seamless tube specifications.
Q: How is C11000 hardened?
Only by cold work, since the grade contains no alloying element that responds to precipitation hardening; annealing is used to soften it again.