Mar 27, 2025 Leave a message

C10200 Oxygen-Free Copper: The Key Metal Behind Precision Electronics Manufacturing

Why Purity Is the First Requirement in Precision Electronics

Precision electronics manufacturing has moved toward tighter feature sizes, higher switching frequencies and longer service intervals, and each of those trends pushes the same demand onto the materials inside the package. C10200 oxygen-free copper answers that demand because its copper content is 99.95% minimum and its residual oxygen is held at or below 0.001%, so impurity scattering inside the lattice is small and the metal behaves predictably.

The absence of oxygen is the critical detail. Tough pitch copper carries cuprous oxide particles at the grain boundaries; when such material is brazed, welded or annealed in a hydrogen-bearing atmosphere, the oxide reduces and the boundaries open up, producing the classic steam embrittlement failure. C10200 removes that mechanism entirely, which matters because most precision components pass through at least one high-temperature joining step before they are assembled.

Conduction and Thermal Management Performance

C10200 reaches electrical conductivity of 100–101% IACS, and its thermal conductivity sits in the 390 to 401 W/(m·K) band depending on temper. In a device that must move both current and heat, those two numbers decide how small a conductor can be made before losses or temperature rise become unacceptable.

Property Typical Value
Copper content 99.95% minimum
Oxygen content ≤0.001%
Electrical conductivity 100–101% IACS
Thermal conductivity 390–401 W/(m·K)
Density 8.94 g/cm³
Melting point 1083 °C
Modulus of elasticity about 117 GPa

The practical consequence is thermal management by conduction. Where a sealed module cannot be cooled by air, a C10200 heat spreader, heat pipe wall or busbar can carry heat to a chassis-mounted sink with a temperature drop of only a few degrees per 100 mm of path length.

Formability, Corrosion Resistance and Long-Term Stability

The grade is highly ductile in the annealed condition, which allows deep drawing, stamping, coining, swaging and fine wire drawing without intermediate anneals. Strip can be rolled to foil thickness for flexible circuits and shielding, and the same metal can be formed into complex connector shells with a single set of tooling.

Ductility: elongation of 40% or more in soft temper supports severe forming operations and tight bend radii.

Corrosion resistance: stable in air, fresh water, sea water in moderate flow conditions and mildly corrosive industrial atmospheres, with a protective surface film that slows further attack.

Non-magnetic behaviour: no interference with magnetic sensors, transformers or instrument pickups.

Surface quality: a clean, oxide-lean surface takes plating, bonding and ultrasonic welding consistently.

Combined with low creep at normal service temperatures, these properties give electronics a material whose electrical and dimensional behaviour remains essentially unchanged over a long product life, reducing the maintenance and replacement burden that follows any drift in contact resistance.

Supply Forms and the Standards That Cover Them

Form Typical Size Range Governing Standard
Strip and sheet 0.2 mm to 6 mm thick, 100–1500 mm wide ASTM B152
Plate 6 mm to 50 mm thick ASTM B152
Foil 0.005 mm to 0.2 mm thick ASTM B370 / B101
Tube 3–300 mm outside diameter ASTM B75, B88, B280
Bar and rod 3–200 mm diameter ASTM B187
Wire 0.05–12 mm diameter ASTM B1, B2, B3

Tempers are designated under ASTM B601, from soft annealed through quarter-hard, half-hard and hard to spring, and the chosen temper determines both the achievable conductivity and the forming behaviour. Strip for deep drawn parts is usually ordered quarter-hard or half-hard; busbar and lead frame stock is normally supplied in a controlled temper that balances stiffness against insertion loss.

Applications and Selection Points

High-frequency connectors, relays and semiconductor lead frames where signal integrity depends on consistent conductor purity.

Conductive busbars and heat dissipation modules in inverters, battery packs and electric drive systems.

Rolled copper foil for flexible circuits and shielding, produced from oxygen-free strip.

Cryogenic and vacuum hardware where ductility must be retained at low temperature.

When specifying, state the product form, temper, dimensional tolerances and the governing standard, and require the oxygen content to be reported by a fusion or equivalent analytical method rather than inferred from conductivity. Certificates traceable to the heat number, together with dimensional and surface inspection records, are what allow a component to be released without further incoming testing.

The direction of the market is clear: thinner conductors, higher frequencies and more compact thermal paths. All three favour an oxygen-free base grade, and C10200 remains the reference material against which alternative selections are compared.

Frequently Asked Questions

Q: Why not use C11000 tough pitch copper instead?
C11000 is cheaper and adequate for many static conductors, but it contains oxygen. Any hydrogen-bearing furnace step, brazing operation or vacuum anneal can then cause grain-boundary cracking, so precision components are usually specified in an oxygen-free grade.

Q: How does C10200 compare with C10100?
C10100 has the higher purity, at 99.99% copper, and slightly better conductivity. C10200 at 99.95% covers most electronics, power and thermal duties at lower cost, and the two are often used side by side in the same assembly.

Q: Can C10200 be plated?
Yes. Its clean, oxide-lean surface takes electrolytic nickel, tin and silver plating reliably, provided the surface is degreased and lightly activated before plating.

Q: Does the temper change the conductivity?
It changes it slightly. Cold work raises tensile strength and reduces conductivity by a small margin, so the conductivity value should always be quoted for the temper that is actually delivered.

Q: What thickness of foil can be produced?
Rolled foil is normally supplied between 0.005 mm and 0.2 mm, and electrodeposited foil can also be produced for laminates that need very fine line widths.

Q: How should the material be stored?
Keep it dry and away from chlorides, in original protective packing with cut ends capped. Copper forms a protective surface film naturally, but prolonged contact with wet masonry or salt-laden air will stain the surface.

Send Inquiry

whatsapp

Phone

E-mail

Inquiry