Designations and Scope of the Grade
C10200 is the UNS designation for oxygen-free copper, sometimes written as OF-Cu in commercial correspondence and as Cu-OF in international designation systems. In Europe the grade is numbered CW008A under EN 1412, in Japan it appears as C1020, and in the Chinese system as TU2. All of these designations point to the same material: wrought copper with 99.95% minimum copper and an oxygen content limited to 0.001% maximum.
The distinction between this grade and ordinary high-conductivity tough pitch copper is metallurgical rather than cosmetic. Tough pitch copper carries its oxygen as dispersed cuprous oxide; C10200 carries essentially none, so it can be processed in reducing atmospheres and used in sealed devices without the risk of internal cracking.
Specification Limits
| Parameter | Limit | Reason for the limit |
|---|---|---|
| Copper (Cu), including silver | 99.95% minimum | Sets the conductivity ceiling |
| Oxygen (O) | 0.001% maximum | Prevents hydrogen embrittlement |
| Total impurities excluding Cu and Ag | 0.05% maximum | Keeps resistivity low |
| Flat rolled products | ASTM B152 | Sheet, strip, plate and rolled bar |
| Rod and bar | ASTM B124 | Bar, rod and shapes |
| Seamless tube | ASTM B68, ASTM B188 | Tube for general and electrical service |
Physical and Mechanical Properties
| Property | Typical value | Test reference |
|---|---|---|
| Electrical conductivity | 100% IACS minimum (58 MS/m) | ASTM E1004 |
| Electrical resistivity | 1.724 micro-ohm-cm at 20 C | ASTM B193 |
| Thermal conductivity | about 390 W/(m K) | ASTM E1461 |
| Density | 8.94 g/cm³ | Gravimetric |
| Melting point | 1083 C | Pure metal constant |
| Specific heat capacity | 0.385 J/(g K) | Calorimetry |
| Elastic modulus | 117 GPa | ASTM E111 |
| Annealed tensile strength | 200-250 MPa | ASTM E8/E8M |
| Annealed hardness | about 40-50 HV | ASTM E18 conversion |
Mechanical values are temper dependent. Soft annealed material is chosen when forming dominates, while H02 and harder tempers are specified for current-carrying parts that must keep their shape under mechanical load. Because no alloying element is present, the strength range available from this grade is narrower than that of a precipitation-hardening copper.
Heat Treatment and Fabrication
Annealing. Soft annealing is carried out in the 375-650 C range, normally in a protective atmosphere, with time selected to complete recrystallisation without excessive grain growth.
Hot working. The practical hot working window lies between roughly 700 C and 900 C; overheating risks coarse grains, which reduce fatigue performance.
Cold working. Drawing, rolling and stamping are straightforward. Reductions above 80% between anneals are normal, and the metal tolerates tight bend radii in the soft condition.
Joining. Soft soldering, silver brazing and resistance welding all succeed. Fusion welding needs care because the absence of deoxidising additions makes the weld pool sensitive to porosity.
Cleaning. Degrease and lightly pickle before plating or vacuum service; residual rolling lubricant is a common source of outgassing complaints.
Where the Grade Is Used
Electro-vacuum equipment is the classic application. High power transmitter tubes, magnetrons, vacuum capacitors and interrupter contacts use C10200 because an intergranular crack in these components would destroy the vacuum seal and end the service life of the device. In electronics and electrical engineering, the grade appears as high-frequency coaxial inner conductors, transistor and lead frame stock, busbars and winding strip, where the low resistivity keeps losses and temperature rise to a minimum. Heat exchanger and cold plate manufacture uses the thermal conductivity of about 390 W/(m K) to move heat away from power electronics. Chemical plant, high temperature process equipment and architectural components take advantage of the corrosion behaviour of pure copper in neutral and mildly oxidising environments.
FAQ
Q: What does OF-Cu mean?
OF stands for oxygen-free and Cu is the chemical symbol for copper; OF-Cu is the commercial way of naming the same grade that the UNS system lists as C10200.
Q: How does C10200 differ from C11000?
C11000 is electrolytic tough pitch copper with oxygen in the range of about 0.02-0.04%, while C10200 limits oxygen to 0.001% and is therefore the choice for vacuum and reducing-atmosphere service.
Q: Can this grade be hardened by heat treatment?
No. Being essentially pure copper it cannot be strengthened by precipitation, so hardness is adjusted by cold work and controlled by annealing.
Q: Why is the grade preferred for vacuum devices?
It has no oxide inclusions to release gas under vacuum and no oxide to react with hydrogen, so seals remain leak tight.
Q: What is the recommended annealing range?
Soft annealing is performed between 375 C and 650 C in a protective atmosphere, with the exact cycle matched to gauge and required grain size.
Q: Which test proves the oxygen limit has been met?
Inert gas fusion analysis on a sample from the heat, supported by metallographic examination for cuprous oxide where a client specification requires it.