C10200 Copper Alloy: Definition and Scope
C10200 is the UNS designation for oxygen-free copper (OF copper), a wrought high-purity copper grade produced so that the residual oxygen content of the melt is kept at an extremely low level. In ordinary electrolytic tough pitch copper the oxygen is present as dispersed cuprous oxide particles; in C10200 those particles are essentially absent, which changes both the metallurgical behaviour and the processing window of the material.
The practical consequence is that C10200 can be brazed, welded, annealed or otherwise exposed to hydrogen-bearing atmospheres without the internal cracking known as hydrogen embrittlement. Steam from the reaction between hydrogen and cuprous oxide is the usual cause of that failure mode, and it simply cannot form in a genuinely oxygen-free structure.
Chemical Composition and Applicable Standards
C10200 is specified in ASTM B152 for copper sheet, strip, plate and rolled bar, and the same grade is covered in ASTM B124 for rod and bar, ASTM B188 and ASTM B68 for seamless tube, and ASTM B170 for wire. In the European system the corresponding designation is CW008A under EN 1412, in the Japanese system C1020, and in the Chinese system TU2 under GB/T 5231. The compositional requirements below are the limits common to the ASTM and EN specifications.
| Element | Requirement | Function |
|---|---|---|
| Copper (Cu), incl. silver | 99.95% minimum | Base metal; controls conductivity |
| Oxygen (O) | 0.001% maximum | Held low to prevent hydrogen embrittlement |
| Silver (Ag) | 0.0025% maximum (counted in Cu) | Traced impurity, no separate addition |
| Phosphorus (P) | 0.0003% maximum | Residual only; high P would cut conductivity |
| Total other impurities | 0.05% maximum | Sum of all elements other than Cu and Ag |
Physical and Mechanical Properties
Because the grade is essentially pure copper, its physical constants are those of the pure metal rather than of a diluted alloy. Mechanical values depend strongly on temper, so a purchase specification should always name the temper in addition to the UNS number.
| Property | Typical value | Remark |
|---|---|---|
| Electrical conductivity | 100% IACS (58 MS/m) minimum | Meets or exceeds annealed copper standard |
| Electrical resistivity | 1.724 micro-ohm-cm at 20 C | Per ASTM B193 test method |
| Thermal conductivity | about 390 W/(m K) | Core advantage in heat transfer hardware |
| Density | 8.94 g/cm³ | Used for mass-to-volume conversion |
| Melting point | 1083 C | Narrow solidification range |
| Annealed tensile strength | typically 200-250 MPa | O60/O61 soft temper |
| Annealed elongation | typically 40% and above | Confirms suitability for deep drawing |
Temper designations follow the usual wrought-copper system: O60 or O61 for soft annealed, H01 and H02 for quarter-hard and half-hard, and H04 to H08 for progressively cold worked conditions. Cold work raises tensile strength and hardness at the cost of elongation and, to a small extent, conductivity.
Processing and Fabrication Characteristics
C10200 is regarded as one of the most forgiving copper grades to fabricate. It can be hot rolled between roughly 700 C and 900 C, cold rolled and drawn with heavy reductions, deep drawn and stamped, and forged into fittings and electrical hardware. Because the material is soft, tooling must be kept sharp and surface contact points protected to avoid mechanical scratching of the finished surface.
Cold forming: excellent; reductions above 80% are routinely achieved with intermediate annealing.
Annealing: soft anneal in the 375-650 C range in a protective or reducing atmosphere.
Joining: soft soldering, silver brazing and resistance welding all perform well; fusion welding is possible but requires attention to porosity control.
Machining: free-cutting behaviour is moderate because no lead or sulphur is present; carbide tooling with generous coolant is preferred.
Surface protection: bright annealed or tinned finishes are common where stored stock must not oxidise.
Applications and Selection Guidance
The conductivity and cleanliness of C10200 make it a first choice wherever current density, signal integrity or vacuum tightness are critical. Typical uses include busbars and switchgear conductors, transformer windings, high-frequency coaxial cable inner conductors, lead frames and connector stock, vacuum interrupters and transmitter tubes, heat exchanger and cold plate components, and acoustic or decorative parts that are later plated.
When selecting the grade, confirm three points: the oxygen limit that your joining process actually requires, the temper that delivers the required yield strength, and the surface finish that downstream plating or bonding demands. Where higher strength is essential, a dilute alloy such as a silver-bearing copper or a precipitation-hardening grade should be considered instead, since C10200 achieves its properties from purity rather than from alloying.
FAQ
Q: What does "oxygen-free" mean for C10200?
It means the oxygen content is held to 0.001% maximum, so essentially no cuprous oxide particles remain in the structure and hydrogen embrittlement cannot occur.
Q: Is C10200 the same as C11000?
No. Both are high-conductivity coppers, but C11000 is electrolytic tough pitch copper containing roughly 0.015-0.040% oxygen, while C10200 is oxygen-free and is preferred for vacuum and reducing-atmosphere service.
Q: Which standards cover C10200 products?
ASTM B152 for sheet, strip, plate and rolled bar; ASTM B124 for rod and bar; ASTM B68 and B188 for seamless tube; ASTM B170 for wire. Equivalent designations are CW008A under EN 1412, C1020 under JIS, and TU2 under GB/T 5231.
Q: Can C10200 be welded?
It can be soldered, brazed and resistance welded without difficulty. Fusion welding is feasible but demands clean joint preparation and controlled shielding because the material has no deoxidising additions.
Q: How is oxygen content verified?
By inert gas fusion or by the standard metallographic examination for cuprous oxide, normally performed once per heat on a sample taken from the cast or rolled product.
Q: What tempers are normally stocked?
Soft annealed O60/O61 strip and sheet, quarter-hard and half-hard tempers for connector stock, and spring tempers for small electrical parts.