Dec 29, 2025 Leave a message

Brass C26000 Equivalent Grades: C2600, CW508L, CuZn30 and H68

What Is C26000 Brass?

C26000 is the UNS designation for the alloy commonly called cartridge brass or 70/30 brass - a single-phase alpha brass containing nominally 70 % copper and 30 % zinc. It is the most ductile of the ordinary copper-zinc alloys and combines that ductility with good strength, so it can be deep drawn, spun and cold formed to a degree that the higher-zinc brasses cannot match. Typical products are sheet, strip, plate, bar, rod and drawn tube.

The alloy has excellent resistance to atmospheric and fresh-water corrosion and is widely used in electrical and hardware applications. It is, however, not suitable for service with acetic acid, moist ammonia or ammonia compounds, hydrochloric acid or nitric acid, all of which attack the alloy rapidly. Ammonia and its compounds are of particular concern because they cause stress-corrosion cracking in material that has been cold worked.

Equivalent Designations Across Standards

The table below compares the C26000 designation with the equivalent numbers used in other national and international systems. These are compositional equivalents, not automatic approvals: a designer substituting one for another must still verify composition tolerances, temper and the applicable product specification.

System Designation Remarks
UNS (USA) C26000 Primary universal designation
ASTM (USA) B36, B134, B135 Sheet, strip and tube product specifications
SAE (USA) CA260 Older automotive and aerospace designation
CDA (USA) 260 Copper Development Association numbering
EN (Europe) CW508L Material number CuZn30
ISO CuZn30 International designation
DIN (Germany) CuZn30 (2.0265) Widely cited in European engineering
BS (UK) CZ108 / CZ109 British Standard 70/30 brass
JIS (Japan) C2600 Japanese Industrial Standard - one digit shorter
GB (China) H68 Traditional Chinese designation, still in common use
GOST L68 Cyrillic designation for the same composition

Common trade names are cartridge brass and 70/30 brass. Because the JIS number C2600 differs from the UNS number C26000 by a single digit, purchase orders should always spell out whether the American or the Japanese system is intended.

Chemical Composition

The composition limits below follow the C26000 specification. Copper plus the sum of the named elements must be at least 99.7 %.

Element Limit
Copper (Cu) 68.5 – 71.5 %
Lead (Pb) 0.07 % max
Iron (Fe) 0.05 % max
Zinc (Zn) Remainder

Lead is held to a very low maximum because it embrittles the hot-working range of the alloy and reduces ductility. Grades intended for potable-water contact are subject to separate lead-leaching requirements in the relevant national regulation, and for drinking-water fittings the alloy may need to be replaced by a low-lead alternative.

Physical and Fabrication Properties

Property Typical value
Melting range (solidus – liquidus) 915 – 955 °C (1680 – 1750 °F)
Density 8.53 g/cm³ (0.308 lb/in³) at 20 °C
Specific gravity 8.53
Electrical conductivity 28 % IACS at 20 °C
Thermal conductivity about 120 W/m·K (70 Btu/ft²/ft/h/°F) at 20 °C
Coefficient of thermal expansion 20 × 10⁻⁶ per °C over 20 – 300 °C
Specific heat capacity 0.38 kJ/kg·K at 20 °C
Modulus of elasticity in tension about 110 GPa (16 × 10⁶ psi)
Modulus of rigidity about 41 GPa (6 × 10⁶ psi)

Mechanically, C26000 can be supplied from the annealed condition, with a tensile strength around 300 – 340 MPa and elongation above 40 %, right through the hard tempers used for strip and spring components. The alloy work-hardens readily, so intermediate anneals are needed between deep-drawing passes.

Fabrication technique Suitability
Soldering Excellent
Brazing Excellent
Oxy-acetylene welding Good
Gas-shielded arc welding Good
Coated-metal arc welding Not recommended

Soldering and brazing are the preferred joining methods; fusion welding is possible but generates zinc fume and a coarser grain structure in the heat-affected zone, so it is normally reserved for non-critical joints. Where fusion welding is unavoidable, the assembly should be stress-relieved afterwards to reduce the risk of stress-corrosion cracking in service.

Applications and Substitution Notes

Typical uses include ammunition cartridge cases (the origin of the name), electrical connectors and terminals, radiator cores, hardware, fasteners, lock components, hinges, drawn and spun holloware, and architectural trim.

When substituting an equivalent grade it is not enough to compare copper content. Confirm the following: the product specification that applies to the form being bought; the temper and the resulting mechanical properties; the lead limit if the part touches drinking water; and whether the part will be cold formed and then exposed to ammonia-bearing atmospheres, in which case a stress-relief anneal may be required. A grade that matches on composition but not on temper can fail in a deep-drawing press or in stress-corrosion service.

FAQ

Q: Is C26000 the same as C2600?
C26000 is the UNS designation used in the United States; C2600 is the Japanese Industrial Standard designation. They describe the same 70/30 brass composition, but the standard number, tolerance tables and test requirements differ, so the applicable specification must be stated.

Q: What is the European equivalent of C26000?
The EN designation is CW508L with the material designation CuZn30, formerly listed as DIN 2.0265. It is compositionally equivalent and is the grade most often quoted by European fabricators.

Q: What is H68 brass?
H68 is the Chinese designation for the same 70 % copper, 30 % zinc alloy. The letter H denotes brass (huang tong) and 68 indicates the nominal copper content, which is slightly lower than the 70 % implied by the American trade name.

Q: Can C26000 brass be welded?
It can be joined by gas-shielded arc welding and oxy-acetylene welding, but fusion welding produces zinc fume and a coarse heat-affected zone. Soldering and brazing give better results and are the usual production methods.

Q: Is C26000 suitable for marine or ammonia service?
No. The alloy is not recommended for sea-water immersion and is attacked by moist ammonia and ammonium compounds, which cause stress-corrosion cracking in cold-worked parts. Choose a copper-nickel alloy for marine duty.

Q: What tempers are stocked for C26000 sheet and bar?
Annealed, quarter-hard, half-hard, three-quarter-hard and hard tempers are standard for sheet and strip; bar and rod are supplied in drawn or extruded-and-drawn tempers. The temper controls the balance between formability and strength.

Summary for Buyers

C26000 cartridge brass sits at the ductile end of the brass family, which is why it is still the default choice for deep-drawn and cold-formed parts. When an equivalent grade is offered, match the standard, the temper and the lead limit - not just the copper content - and remember that JIS C2600 and UNS C26000 are different designations for the same alloy under different rules.