ASTM B111 C68700 is the aluminum brass seamless tube grade specified for heat exchanger tube bundles in seawater-cooled condensers, evaporators and distillers. The alloy contains 76.0-79.0% copper and 1.8-2.5% aluminum with a controlled arsenic addition of 0.02-0.06%. Aluminum forms a thin, self-repairing oxide film that resists high-velocity salt water and polluted harbour water, while arsenic suppresses preferential loss of zinc. The same material appears internationally as CuZn20Al2As, HAL77-2 in GB/T 8890, CZ110 in BS 2871, C6870 in JIS H3300 and CuZn20Al2 in DIN 1785.
What a C68700 Tube Bundle Consists Of
A tube bundle is the assembled heat transfer surface of a shell-and-tube exchanger: the set of seamless tubes together with the tube sheets, baffles and tie rods that locate them. A C68700 bundle can be supplied as straight tubes, or as U-shaped tubes bent from the same production heat, so that the complete bundle is fabricated, heat treated and tested as one unit before dispatch. Straight tubes ship in the O61 annealed temper. U-bend tubes are formed after the final anneal and are ordered to the dimensional and bending requirements of the U-bend specification ASME SB395, which is used alongside ASTM B111 for this product form.
Typical bundle configurations:
Tube outside diameter: 15 mm to 25 mm
Wall thickness: 0.5 mm to 1.2 mm
Length: up to 6000 mm
Tube arrangement: straight or U-shaped
Tubes are produced to close tolerances, typically plus or minus 0.05 mm on outside diameter and plus or minus 10% on wall thickness. Tolerance control matters because tube-to-tube-sheet expansion works inside a narrow band: over-rolling a thin wall distorts the ligament between holes, while under-rolling leaves a potential leak path along the joint.
Chemical Composition and Mechanical Properties
Table 1. Composition and room-temperature properties of UNS C68700 in the O61 annealed temper, as required by ASTM B111.
| Copper, Cu | 76.0-79.0% |
| Aluminum, Al | 1.8-2.5% |
| Arsenic, As | 0.02-0.06% |
| Iron, Fe | 0.06% max |
| Lead, Pb | 0.07% max |
| Zinc, Zn | remainder |
| Tensile strength, min | 345 MPa (50 ksi) |
| Yield strength, min | 125 MPa (18 ksi) |
| Temper | O61, annealed |
| Density | 8.33 g/cm³ (0.301 lb/in³) |
| Melting range | 932-971 °C |
ASTM B111 sets minimum tensile strength, minimum yield strength and minimum elongation for every UNS number and temper combination. The annealed O61 temper is the delivery condition for condenser and heat exchanger tube, and the mechanical test certificate of each lot states the measured values against those minimums, so the buyer can confirm that the bundle has not been supplied in a harder, less expandable temper.
Corrosion and Thermal Behaviour in Service
Seawater corrosion rate: below 0.01 mm/year in clean, flowing seawater, with the protective aluminum oxide film re-forming after light mechanical damage.
Velocity tolerance: aluminum brass is chosen specifically for high-velocity and turbulent cooling water, where low-alloyed brasses would suffer erosion-corrosion at the tube inlet.
Fouling behaviour: the controlled release of copper ions limits macrofouling of the tube bore, which helps the overall heat transfer coefficient stay stable between cleaning cycles.
Thermal conductivity: 100.4 W/(m·K) at 20 °C, far above stainless steel, so thin walls can be used without sacrificing heat transfer.
Coefficient of linear expansion: 18.5 × 10-6 per °C over 20-300 °C.
Specific heat capacity: 0.09 cal/(g·°C) at 20 °C.
Inspection and Testing of Finished Bundles
Each tube passes a defined test sequence before a bundle is released:
Eddy current testing of the full tube length to Practice E243, to detect surface and subsurface discontinuities.
Hydrostatic testing at 1.5 times the design pressure, or to the fibre stress stated in ASTM B111 where the standard sets the governing minimum.
Expansion test to Test Method B153 and flattening test on samples from the lot; both must show no visible cracks or ruptures.
Residual stress test: C68700 is one of the alloys for which ASTM B111 requires the mercury nitrate test (B154) or the ammonia vapour test (B858).
Material test certificate recording heat number, chemical analysis, mechanical properties and non-destructive test results.
Service Applications
Shipbuilding: main and auxiliary condensers, lubricating oil coolers and jacket water coolers on commercial and naval vessels.
Offshore platforms: seawater cooling circuits and process heat exchangers exposed to continuous salt spray.
Coastal power plants: steam surface condensers operating on once-through seawater cooling.
Desalination plants: distiller and evaporator tube bundles in multi-stage flash and multi-effect trains, where the tube must tolerate brine at elevated temperature.
Selection and Handling Notes
Three factors decide whether a C68700 bundle reaches its design life. First, cooling water chemistry: sulphide-bearing or ammonia-contaminated water attacks the protective film, and in such service the allowable velocity window narrows sharply. Second, velocity profile: the tube inlet and the U-bend outer crest are the most erosion-prone zones, so inlet-end inserts or protective coatings are common on high-velocity units. Third, mechanical support: baffle spacing, tube sheet hole clearance and U-bend ovality all influence vibration fatigue, and tubes should be stored dry, capped and free of standing water before installation.
FAQ
Q: What is ASTM B111 C68700?
ASTM B111 is the specification for seamless copper and copper-alloy condenser tubes and ferrule stock. C68700 is the aluminum brass grade within it, containing 76.0-79.0% copper, 1.8-2.5% aluminum and 0.02-0.06% arsenic, normally supplied in the O61 annealed temper.
Q: What are the minimum mechanical properties of C68700 in the O61 temper?
345 MPa (50 ksi) minimum tensile strength and 125 MPa (18 ksi) minimum yield strength. The elongation minimum is specified by ASTM B111 for each UNS number and temper, and is verified on the test certificate supplied with the lot.
Q: How does C68700 compare with C44300 admiralty brass?
C44300 contains 70.0-73.0% copper with 0.9-1.2% tin and 0.02-0.06% arsenic, and performs well in clean seawater. C68700 replaces tin with aluminum, which raises annealed strength and gives markedly better resistance to high water velocity, making it the usual choice for once-through coastal condensers.
Q: Which standards list equivalent C68700 grades?
GB/T 8890 designates it HAL77-2, BS 2871 uses CZ110, JIS H3300 lists C6870, DIN 1785 uses CuZn20Al2, and the ASME counterpart of ASTM B111 is SB111. The U-bend form is covered by ASTM B395 and ASME SB395.
Q: Why is arsenic added to aluminum brass tube?
The 0.02-0.06% arsenic addition acts as a cathodic inhibitor that prevents preferential dezincification of the brass matrix, which is the main failure mode of plain brass in aerated or low-velocity water.
Q: How is a C68700 tube bundle tested before shipment?
Eddy current testing of the full length, hydrostatic testing, expansion and flattening tests on lot samples, and the residual stress test required for this alloy, all supported by a material test certificate for each heat.