ASTM B111 C68700 in Heat Exchanger Service
ASTM B111/B111M is the standard specification for seamless copper and copper-alloy condenser tubes and ferrule stock, and C68700 aluminium brass is one of its most widely used grades. Within a heat exchanger, the tube is the component that separates two fluids while carrying heat between them, so the material has to satisfy three requirements at once: it must conduct heat efficiently, it must survive the corrosive side of the exchanger, and it must be formable enough to be bent and rolled into the tube sheet without damage.
Aluminium brass meets all three. Its thermal conductivity is high for a copper alloy, its aluminium-rich surface film resists flowing seawater, and its annealed condition has the ductility needed for U-bending and tube sheet expansion. That combination is why it appears in power plant condensers, refinery coolers, desalination plant and shipboard machinery.
Composition and Cross-Standard Equivalents
The grade is known by a different designation in almost every standard system, and buyers comparing quotations need to match them carefully because the composition ranges are not identical.
| Standard system | Designation | Copper range | Aluminium range | Arsenic range |
|---|---|---|---|---|
| ASTM B111 (UNS) | C68700 | 76.0-79.0 % | 1.8-2.5 % | 0.02-0.06 % |
| BS 2871 Part 3 | CZ110 | 76.0-78.0 % | 1.8-2.3 % | 0.02-0.06 % |
| DIN 1785 | CuZn20Al2 (2.0460) | 76.0-79.0 % | 1.8-2.3 % | 0.02-0.35 % |
| EN | CW702R | 76.0-79.0 % | 1.8-2.5 % | 0.02-0.06 % |
| JIS H3300 | C6870 | 76.0-79.0 % | 1.8-2.5 % | 0.02-0.06 % |
| GB/T 5231 | HAl77-2 | 76.0-79.0 % | 1.8-2.5 % | 0.02-0.06 % |
Two practical differences are worth noting. First, the arsenic range in the German designation is much wider than in ASTM B111, so a tube made to the German grade is not automatically compliant with the ASTM chemistry. Second, national standards set their own mechanical property requirements and temper designations, so the temper and its tensile minimum, not just the alloy name, must be quoted when comparing offers.
Thermal and Mechanical Performance
| Property | Value | Comment |
|---|---|---|
| Density | 8.33 g/cm³ | 0.301 lb/in³ at 20 C |
| Thermal conductivity | About 100 W/(m K) | High for a corrosion resistant alloy |
| Electrical conductivity | About 23 % IACS | Annealed condition |
| Elastic modulus | 117 GPa | Room temperature |
| Melting range | Approximately 900-930 C | Safe for brazed joints at normal temperatures |
| Specific gravity | 8.33 | Consistent with the density above |
Mechanically, ASTM B111 requires a minimum tensile strength of 345 MPa and a minimum yield strength of 125 MPa in the annealed O61 temper, which is the normal supply condition for U-bend heat exchanger tube. Hard drawn tube is available where the exchanger works at higher pressure and the tubes are straight. Because heat transfer performance depends on wall thickness, the practical choice of 0.9 mm, 1.2 mm or heavier wall is usually made from corrosion allowance rather than from strength, and the ordering specification should always state outside diameter, wall thickness, length, temper and test requirements explicitly.
Where the Alloy Performs Best
Seawater cooled shell and tube heat exchangers in refineries and chemical plants
Surface condensers in steam power generation
Desalination and distillation plant tube bundles
Marine and offshore machinery coolers and evaporators
HVAC and refrigeration condensers operating on brackish or chlorinated water
Feedwater heaters and other low to medium temperature heat transfer duties
The alloy's natural fouling resistance is an advantage in seawater service, since less biological growth means a smaller loss of heat transfer and longer intervals between cleanings. Where the water is heavily polluted, contains sulphides or reaches higher temperatures, copper-nickel grades such as C70600 and C71500 give longer life, and where the water is clean fresh water at moderate temperature, admiralty brass offers a lower cost solution.
Ordering, Installation and Testing Points
Ordering should state the UNS number or the national equivalent, the temper, the outside diameter and wall thickness with tolerances, the length or U-bend drawing, the test schedule and any additional requirements such as eddy current examination or grain size limits. Tube ends are commonly supplied with protective caps or ferrules, and packaging must keep the tubes dry, separated and free of chloride-bearing residues during sea transport.
During erection, tubes are rolled into the tube sheet with controlled expansion, and baffle spacing is checked so that tubes cannot vibrate against one another. Water side cleaning should use inhibited chemicals, brushes or water jetting only. The final inspection of the bundle typically includes hydrostatic or pneumatic testing, eddy current examination of the installed tubes and a check on the expansion joint quality, all of which depend on the tube having arrived with the correct temper and surface condition.
FAQ
Q: What is the Chinese equivalent of C68700 tube?
The nearest Chinese designation is HAl77-2 under GB/T 5231, with an aluminium content of about 2 % and a small arsenic addition for dezincification resistance.
Q: What temper is used for U-bend heat exchanger tubes?
Annealed O61 tube is used because it has the ductility required for bending and for rolling into the tube sheet without cracking.
Q: Does C68700 tube conduct heat well?
Yes, its thermal conductivity of roughly 100 W/(m K) is high for a seawater resistant copper alloy, although it is below that of pure copper and of the admiralty brasses.
Q: Can a tube made to DIN CuZn20Al2 be used where ASTM B111 C68700 is specified?
Not automatically, because the arsenic range permitted in the German designation is wider, so the chemistry should be verified against the ASTM limits before the tube is accepted.
Q: How much corrosion allowance should be added to the wall thickness?
The allowance follows from the water chemistry, velocity and expected service life; it is normal to specify a heavier wall in aggressive seawater rather than to rely on the alloy alone.
Q: What tests are required on C68700 heat exchanger tube?
Typical requirements are chemical analysis, tensile and hardness testing, dimensional and surface inspection, expansion and flattening tests, hydrostatic pressure testing and eddy current examination of the full length.