What ASTM B111 C10100 Oxygen-Free Copper Tube Is
ASTM B111/B111M is the specification for seamless copper and copper-alloy condenser tubes, ferrule stock and U-bends used in heat exchangers, condensers, evaporators and similar heat-transfer equipment. UNS C10100, also designated Cu-OFE, is the highest-purity wrought copper grade in that family: copper content is 99.99 percent minimum and oxygen is held to 0.0005 percent maximum, while phosphorus, sulphur and other residuals are restricted to trace levels.
Because almost all residual oxygen is removed, C10100 tube resists hydrogen embrittlement when it is heated in a reducing or hydrogen-bearing atmosphere, and it does not develop internal oxide films during high-temperature brazing. That combination of purity, conductivity and metallurgical stability is why the grade is selected for exchangers that also have to meet strict cleanliness, vacuum or semiconductor requirements.
Composition and Specification Overview
| Item | Requirement |
|---|---|
| Copper (Cu), including silver | 99.99 % minimum |
| Oxygen (O) | 0.0005 % maximum |
| Phosphorus, sulphur and other residuals | individually controlled to trace levels |
| Product standard | ASTM B111/B111M, ASME SB111 |
| Tempers | O60 soft annealed and the drawn tempers listed for the grade |
| Forms | seamless round tube in straight lengths, U-bends, pancake coils, ferrule stock |
| Typical tube sizes | outside diameter 6 mm to 89 mm, wall 0.5 mm to 3.5 mm |
| Verification tests | expansion, flattening, residual stress, eddy current, hydrostatic or pneumatic pressure |
Properties That Drive Grade Selection
ASTM B111 sets minimum tensile strength, yield strength and elongation for each UNS number and temper, together with grain-size limits in the annealed condition. Soft annealed (O60) copper tube of this type is specified at a minimum tensile strength of 207 MPa (30 ksi), with elongation at the high levels typical of fully annealed copper; drawing the tube to a harder temper raises strength at the cost of formability.
| Property | Typical value |
|---|---|
| Density | 8.94 g/cm³ at 20 °C |
| Melting point (liquidus) | 1083 °C |
| Electrical conductivity | 101 % IACS minimum |
| Thermal conductivity | about 390 W/(m·K) at 20 °C |
| Modulus of elasticity | about 117 GPa |
| Coefficient of thermal expansion | 17.0 x 10^-6 per °C (20-100 °C) |
Applications
Power station condensers, feedwater heaters and turbine oil coolers where maximum heat transfer per unit area is required.
Cryogenic and liquefied-gas exchangers, where copper remains ductile at low temperature.
High-vacuum chambers, accelerator components and analytical instruments that cannot tolerate internal oxide or outgassing.
Semiconductor and electronics cooling plates, busbars and high-current conductors.
Medical and laboratory equipment, including steriliser coils and precision heat sinks.
Fabrication and Joining Guidance
Oxygen-free copper tube is ductile in the annealed condition and can be rolled, bent to tight radii and expanded into tube sheets without cracking. Cold work raises strength and lowers ductility, so a full anneal at 250 °C to 650 °C, or a stress relief at 200 °C to 250 °C, is normally applied after severe forming. Hot working is carried out between roughly 750 °C and 950 °C.
Soldering and brazing are the preferred joining methods and both rate as excellent for this grade; because no oxides form at the joint interface, brazing can be performed in reducing-atmosphere furnaces. Where fusion welding is required, gas tungsten arc welding in an inert atmosphere with a matching filler gives clean, sound joints. Cutting should be done with a sharp tool and the tube ends deburred and cleaned before rolling into a tube sheet.
Inspection Points and Common Pitfalls
Eddy-current examination is carried out on the finished tube to detect cracks, laps and inclusions; acceptance limits should be agreed with the purchaser before production.
The expansion and flattening tests verify ductility, and a residual-stress test confirms that straight tube has been properly stress relieved before bending.
Grade confusion is the most frequent problem: C10100 (99.99 % Cu, 0.0005 % O) is not interchangeable with phosphorus-deoxidised C12200 where maximum conductivity is specified.
Contamination during storage is a real risk in high-purity service; tube should be kept dry, capped and free of oil, marking inks and workshop dust.
Bend ovality, wall thinning on the outside of the bend and U-bend leg tolerances must be checked, because they control bundle assembly and later tube expansion.
FAQ
Q: What is the difference between C10100 and C10200 copper tube?
C10100 is the higher-purity oxygen-free grade with 99.99 percent minimum copper and 0.0005 percent maximum oxygen, while C10200 requires 99.95 percent minimum copper at a similar low oxygen level. C10100 is chosen when conductivity and cleanliness requirements are at their most demanding.
Q: Why is oxygen content important in a heat exchanger tube?
Residual oxygen can combine with hydrogen at high temperature and cause internal steam voids and cracking, a failure mode known as hydrogen embrittlement. Keeping oxygen below 0.0005 percent removes that risk and also prevents internal oxide films during brazing.
Q: Which tempers are normally supplied?
Soft annealed O60 tube is standard for U-bends and coils that must be formed after delivery, while drawn tempers are supplied for straight tube that needs higher stiffness. The temper, temper designation and mechanical requirements are stated on the purchase order.
Q: Can C10100 tube be brazed rather than welded?
Yes. Brazing and soldering both rate as excellent for oxygen-free copper, and furnace brazing in a reducing atmosphere is common because no surface oxide forms. Fusion welding is used where a wrought joint of matching strength is needed.
Q: What quality documents normally accompany the tube?
Mill test certificates quoting chemical analysis and mechanical results are issued against the heat number, together with records of eddy-current or pressure testing and dimensional inspection, so that the bundle can be traced through fabrication and commissioning.
Q: How should the tube be stored before installation?
Keep it indoors, dry and capped, in its original protective wrapping, and avoid stacking weights that ovalise the ends. Marking should be done with approved low-halogen pens only, since ink residues can cause corrosion in service.