Scope and Definition of ASME SB111 C68700 O61 Tube
ASME SB111 is the ASME code adoption of ASTM B111/B111M, the specification covering seamless copper and copper alloy condenser tubes and ferrule stock. UNS C68700 is an aluminium brass built on a copper-zinc base to which aluminium and a small deliberate arsenic addition are made. The same material appears in other designation systems as CuZn22Al2 / CW702R (EN 12451), CZ110 (BS 2871 Part 3), C6870 (JIS H3300) and HAl77-2 (GB/T 5231). The O61 suffix is the annealed temper, the condition in which condenser tubes are supplied so that they can be rolled or expanded into a tubesheet without cracking.
The tube is seamless: it is produced by casting, extrusion and cold drawing, so there is no longitudinal weld and no weld-line defect that could open up under thermal cycling. Aluminium in solid solution forms a thin, tenacious surface film that is continually repaired by flowing aerated seawater, while arsenic at 0.02-0.06 % blocks the preferential loss of zinc known as dezincification. This combination is why aluminium brass remains a standard tube material for high-temperature seawater condensers, distillers and multi-stage flash desalination plants.
Chemical Composition and Equivalent Grades
| Element | UNS C68700 (ASTM B111 / ASME SB111) |
|---|---|
| Copper (Cu) | 76.0 - 79.0 % |
| Aluminium (Al) | 1.8 - 2.5 % |
| Arsenic (As) | 0.02 - 0.06 % |
| Iron (Fe) | 0.06 % max |
| Lead (Pb) | 0.07 % max |
| Zinc (Zn) | Remainder |
| System | Designation for C68700 aluminium brass |
|---|---|
| ASTM B111 / ASME SB111 | UNS C68700 |
| EN 12451 | CuZn20Al2As (CW702R) |
| BS 2871 Part 3 | CZ110 |
| JIS H3300 | C6870 |
| GB/T 5231 | HAl77-2 |
| AS 1569 | C68700 |
Dimensions, Tolerances and Delivered Condition
Seamless aluminium brass tube is normally supplied over an outside diameter range of about 6 mm to 300 mm with wall thickness from 0.5 mm to 10 mm, although condenser and heat exchanger work concentrates on the thin-wall band of roughly 12.7 mm to 25.4 mm outside diameter with 0.9 mm to 1.65 mm wall. Straight lengths are commonly 6 m or 12 m, and U-bent or coiled forms are produced for specific exchanger designs. Outside diameter tolerance is tighter for small tubes than for large ones, wall thickness is generally held within 10 % of nominal, and straightness is controlled to about 1 mm per metre so that tubes feed cleanly into tubesheet holes.
Surface: smooth, bright, free from scratches, pits and heavy oxide.
Cleaning: internal and external degreasing before packing.
Heat treatment: annealed (O61) with a light, uniform oxide; stress-relieved conditions on request.
Marking: alloy, size and heat number for full traceability to the mill test certificate.
Packing: bundles in protective wraps or wooden cases for sea freight.
Mechanical, Thermal and Corrosion Behaviour in Service
In the annealed temper C68700 tubing typically shows a tensile strength in the region of 345-460 MPa with yield strength of roughly 125-250 MPa and elongation well above 30 %, which is what allows tubes to be bent, flared and roller-expanded on site. Thermal conductivity is approximately 100 W/(m·K) - high for a copper alloy and the reason aluminium brass is chosen where heat transfer efficiency matters. Density is about 8.33 g/cm³, so tube bundles remain manageable to handle and support.
Seawater resistance: the aluminium-rich film resists impingement and erosion at flow velocities typical of condenser water boxes, and the alloy tolerates chlorination and sulphide-bearing waters better than plain brass.
Dezincification: the arsenic addition raises resistance substantially; performance in this respect is assessed by recognised copper alloy dezincification test methods rather than by ordinary salt spray tests.
Temperature: continuous seawater service is normally considered up to about 250-300 degrees C, comfortably covering condenser and distiller duty.
Ammonia: copper alloys are sensitive to ammonia and ammonium-bearing vapours, so an ammonia environment on the steam side must be evaluated before selection.
Fabrication, Expansion and Welding Guidance
The O61 temper is selected precisely because it deforms readily. Tubes are cut square, deburred and then roller-expanded into the tubesheet: a wall reduction of about 3-5 % gives a sound seal, whereas over-expansion beyond roughly 8 % leaves residual hoop stress that encourages stress corrosion cracking in service. Where tubes are bent into U-form, bend radius should be generous enough to keep ovality within the limits acceptable for the exchanger, and annealing after severe cold forming is normally required.
Aluminium brass is weldable, but arc welding is rarely used for tube joints because the zinc-rich alloy is prone to zinc evaporation and porosity. Where welding is unavoidable, the joint should be made with a matching copper alloy filler in a controlled procedure covering preheat and interpass temperature. Brazing and silver soldering are used for fittings and return bends. After any hot work the assembly should be cleaned and passivated so that the protective aluminium oxide film can reform.
Inspection Points and Common Application Mistakes
Verify that the mill test certificate reports chemistry against ASTM B111 for UNS C68700 - a copper content below 76 % or an arsenic addition outside 0.02-0.06 % defeats the dezincification guarantee.
Eddy current testing is the standard method for confirming seam integrity in thin-wall condenser tubes; hydrostatic or pneumatic testing is used as an alternative or additional check.
Do not mix aluminium brass and copper-nickel tubes in one water box without attention to galvanic effects; dissimilar tube materials and steel water boxes require attention to earthing and cathodic protection.
Store tubes dry and covered. Standing water inside tubes during storage produces oxide staining that is later mistaken for corrosion in service.
Confirm that tube hole clearances in the tubesheet suit the actual outside diameter tolerance of the delivered lot, or expansion will be uneven.
FAQ
Q: What does the O61 temper mean for C68700 tubing?
O61 is the annealed temper called up by ASTM B111. It gives the lowest strength and highest ductility condition, which is what tube expansion, flaring and U-bending require.
Q: Why is arsenic added to aluminium brass?
Arsenic at 0.02-0.06 % is an inhibitor that prevents the selective leaching of zinc from the alloy, greatly extending tube life in aggressive seawater and brackish water.
Q: Can C68700 tubes be used in desalination plants?
Yes. Aluminium brass tubes are widely used in multi-stage flash and other thermal desalination condensers where seawater temperatures and velocities are moderate to high.
Q: How does C68700 compare with copper-nickel tube?
Aluminium brass offers higher thermal conductivity and lower cost, while copper-nickel alloys generally tolerate higher seawater velocities, more severe pollution and higher temperatures. Selection depends on the specific water chemistry and duty.
Q: How are the tubes tested before shipment?
Finished tubes receive dimensional inspection and eddy current examination for seam and wall defects, and mechanical properties are certified from the production heat on the material test certificate.
Q: What causes early tube failure in seawater condensers?